KR101854321B1 - Eco-friendly adhesive composition for bonding finishing foil, and method for manufacturing the same - Google Patents
Eco-friendly adhesive composition for bonding finishing foil, and method for manufacturing the same Download PDFInfo
- Publication number
- KR101854321B1 KR101854321B1 KR1020180001001A KR20180001001A KR101854321B1 KR 101854321 B1 KR101854321 B1 KR 101854321B1 KR 1020180001001 A KR1020180001001 A KR 1020180001001A KR 20180001001 A KR20180001001 A KR 20180001001A KR 101854321 B1 KR101854321 B1 KR 101854321B1
- Authority
- KR
- South Korea
- Prior art keywords
- weight
- parts
- adhesive composition
- bonding
- finishing foil
- Prior art date
Abstract
Description
본 발명은 피니싱 호일 접착용 친환경 접착제 조성물, 그리고 이의 제조 방법에 관한 것으로, 보다 구체적으로는, 목가구용을 포함한 피니싱 호일 접착에 1액형 피니싱 호일 접착용 친환경 접착제 조성물을 적용시 수성 친환경 생산 적용으로 작업 환경이 양호해 지며, 접착제의 2회 도포에서 1회 도포가 가능하므로 라인의 성력화가 가능하도록 하는 피니싱 호일 접착용 친환경 접착제 조성물, 그리고 이의 제조 방법에 관한 것이다. The present invention relates to an eco-friendly adhesive composition for bonding a finishing foil, and more particularly, to an eco-friendly adhesive composition for bonding a finishing foil to a finishing foil including wood furniture, And a method for producing the same, and to an eco-friendly adhesive composition for adhering a finishing foil, which makes it possible to increase the strength of a line by applying the adhesive twice.
현재 합성 수지 필름 및 피니싱 종이 호일용 접찹제는, 기계 작업성, 초기 접착성 등 때문에 2액형 요소 멜라민계 접착제를 사용하고 있다.Currently, two-component urea melamine adhesives are used for adhesives for synthetic resin films and finishing paper foils because of their mechanical workability and initial adhesion.
이에 따라 해당 분야에 있어서는 기존의 접착제를 친환경적이며, 1액형으로 사용이 편리하며, 초기 접착력 등의 품질 특성을 발휘하는 것으로 대체하기 위한 기술 개발이 요구되고 있다.Accordingly, in the related field, it is required to develop a technology for replacing existing adhesives with eco-friendly, one-component type, easy to use, and exhibiting quality characteristics such as initial adhesive strength.
본 발명은 상기의 문제점을 해결하기 위한 것으로, 목가구용을 포함한 피니싱 호일 접착에 1액형 피니싱 호일 접착용 친환경 접착제 조성물을 적용시 수성 친환경 생산 적용으로 작업 환경이 양호해 지며, 접착제의 2회 도포에서 1회 도포가 가능하므로 라인의 성력화가 가능하도록 하기 위한 피니싱 호일 접착용 친환경 접착제 조성물, 그리고 이의 제조 방법을 제공하기 위한 것이다.SUMMARY OF THE INVENTION The present invention has been made to solve the above problems and it is an object of the present invention to provide an environmentally friendly adhesive composition for bonding a one-part finishing foil to a finishing foil including wood furniture, An adhesive composition for bonding a finishing foil, and a method for manufacturing the same.
또한, 본 발명은 친환경적이며, 기존의 Hot Press 공정에 그대로 적용 가능하도록 하기 위한 피니싱 호일 접착용 친환경 접착제 조성물, 그리고 이의 제조 방법을 제공하기 위한 것이다.The present invention also provides an eco-friendly adhesive composition for adhering a finishing foil that is eco-friendly and can be applied as it is to existing hot press processes, and a method for manufacturing the eco-friendly adhesive composition.
그러나 본 발명의 목적들은 상기에 언급된 목적으로 제한되지 않으며, 언급되지 않은 또 다른 목적들은 아래의 기재로부터 당업자에게 명확하게 이해될 수 있을 것이다.However, the objects of the present invention are not limited to the above-mentioned objects, and other objects not mentioned can be clearly understood by those skilled in the art from the following description.
본 발명은, 원재료로 PVAc, PAV, 및 PLA를 준비하되, PVAc : PAV : PLA = 1 : 0.8 내지는 0.9 : 0.2 내지는 0.3의 중량비로 준비한 뒤, PVAc, PAV, 및 PLA가 합해진 전체 중량 100 중량부에 대해서, 발포타입 폴리에틸렌 입자 20 중량부 내지 25 중량부, PHA 수지 1 중량부 내지 10 중량부, 수용성 접착제(methyl cellulose) 3 중량부 내지 20 중량부, 보습제(glcerine) 10 중량부 내지 20 중량부, 그리고 에스테르(drying agent) 2 중량부 내지 5 중량부를 1차 추가 성분으로 첨가하고, 1차 추가 성분이 첨가된 전체 중량 100 중량부에 대해서, 충진제 60 중량부 내지 65 중량부, 그리고 증점제 4 중량부 내지 7 중량부를 2차 추가 성분으로 추가하여 형성되는, 피니싱 호일 접착용 접착제 조성물을 제공할 수 있다.In the present invention, PVAc, PAV and PLA are prepared as raw materials, and PVA, PAV and PLA are mixed together in a weight ratio of PVAc: PAV: PLA = 1: 0.8 to 0.9: 20 to 25 parts by weight of a foamed polyethylene particle, 1 to 10 parts by weight of a PHA resin, 3 to 20 parts by weight of a water-soluble adhesive (methyl cellulose), 10 to 20 parts by weight of a moisturizing agent (glcerine) And 2 parts by weight to 5 parts by weight of a drying agent were added as the first additional components and 60 to 65 parts by weight of the filler and 4 parts by weight of the thickener were added to 100 parts by weight of the total weight added with the first additional component By weight to 7 parts by weight as a second additional component.
본 발명은, 위와 같이 제조된 접착제에 있어, 2차 추가 성분이 추가된 전체 중량 100 중량부에 대해서, 탄소 섬유 24 중량부 내지 25 중량부, 난연제 7 중량부 내지 10 중량부, 자외선차단제 8 중량부 내지 13 중량부, 그리고 표면보호제 2 중량부 내지 3 중량부를 3차 추가 성분으로 추가하고, 3차 추가 성분이 추가된 전체 중량 100 중량부에 대해서, 증류수 30 중량부 내지 40 중량부를 첨가하여 형성되는, 피니싱 호일 접착용 접착제 조성물을 제공할 수 있다.In the present invention, 24 to 25 parts by weight of carbon fiber, 7 to 10 parts by weight of a flame retardant, 8 parts by weight of an ultraviolet screening agent And 13 parts by weight of a surface protecting agent and 2 parts by weight to 3 parts by weight of a surface protective agent were added as a third additional component and 30 parts by weight to 40 parts by weight of distilled water was added to 100 parts by weight of the total weight of the third additional component To provide an adhesive composition for bonding a finishing foil.
본 발명의 실시예에 따른 피니싱 호일 접착용 친환경 접착제 조성물, 그리고 이의 제조 방법은, 목가구용을 포함한 피니싱 호일 접착에 1액형 피니싱 호일 접착용 친환경 접착제 조성물을 적용시 수성 친환경 생산 적용으로 작업 환경이 양호해 지며, 접착제의 2회 도포에서 1회 도포가 가능하므로 라인의 성력화가 가능한 효과를 제공할 수 있다. An eco-friendly adhesive composition for bonding a finishing foil according to an embodiment of the present invention and a method for producing the eco-friendly adhesive composition according to an embodiment of the present invention can be applied to a finishing foil bonding for wood furniture, And it is possible to apply one application in two application of the adhesive, so that it is possible to provide an effect that the line can be enriched.
뿐만 아니라, 본 발명의 다른 실시예에 따른 피니싱 호일 접착용 친환경 접착제 조성물, 그리고 이의 제조 방법은, 원재료가 친환경적이며, 기존의 Hot Press 공정에 그대로 적용 가능한 효과를 제공할 수 있다. In addition, the eco-friendly adhesive composition for bonding a finishing foil according to another embodiment of the present invention and its manufacturing method can provide an effect that the raw material is eco-friendly and can be directly applied to a conventional hot press process.
도 1은 본 발명의 실시예에 따른 피니싱 호일 접착용 친환경 접착제 조성물의 전체적인 제조 과정을 나타내는 흐름도이다.
도 2는 도 1의 피니싱 호일 접착용 친환경 접착제 조성물의 전체적인 제조 과정 중 단계(S10)의 접착제 조성물 제조 과정(S10)을 나타내는 흐름도이다. BRIEF DESCRIPTION OF THE DRAWINGS FIG. 1 is a flow chart showing the overall manufacturing process of an environmentally friendly adhesive composition for bonding a finishing foil according to an embodiment of the present invention. FIG.
FIG. 2 is a flowchart showing an adhesive composition manufacturing process (S10) in step S10 in the entire manufacturing process of the environmentally friendly adhesive composition for bonding the finishing foil of FIG.
이하, 본 발명의 바람직한 실시예의 상세한 설명은 첨부된 도면들을 참조하여 설명할 것이다. 하기에서 본 발명을 설명함에 있어서, 관련된 공지 기능 또는 구성에 대한 구체적인 설명이 본 발명의 요지를 불필요하게 흐릴 수 있다고 판단되는 경우에는 그 상세한 설명을 생략할 것이다.DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, a detailed description of preferred embodiments of the present invention will be given with reference to the accompanying drawings. In the following description of the present invention, detailed description of known functions and configurations incorporated herein will be omitted when it may make the subject matter of the present invention rather unclear.
본 발명의 실시예에 따른 피니싱 호일 접착용 친환경 접착제 조성물은 원재료로 PVAc, PAV, PLA를 1 : 0.8 내지 0.9 : 0.2 내지 0.3의 중량비로 준비한 뒤, PVAc, PAV, PLA 전체 중량 100 중량부에 대해서 발포타입 폴리에틸렌 입자를 20 내지 25 중량부, PHA 수지 1 내지 10 중량부, 수용성 접착제(methyl cellulose) 3 내지 20 중량부, 보습제(glcerine) 10 내지 20 중량부, 에스테르(drying agent) 2 내지 5 중량부를 1차 추가 성분으로 첨가하고, 1차 추가된 전체 중량 100 중량부에 대하여 충진제 60 내지 65 중량부, 증점제 4 내지 7 중량부를 2차 추가 성분으로 추가하고, 2차 추가된 전체 중량 100 중량부에 대하여 탄소 섬유 24 내지 25 중량부, 난연제 7 내지 10 중량부, 자외선차단제 8 내지 13 중량부, 표면보호제 2 내지 3 중량부를 배합하고, 마지막으로 배합물 100 중량부에 대해서 30 내지 40 중량부의 증류수를 첨가하여 형성될 수 있다.The eco-friendly adhesive composition for bonding a finishing foil according to an embodiment of the present invention comprises PVAc, PAV, and PLA in a weight ratio of 1: 0.8 to 0.9: 0.2 to 0.3 as a raw material, 20 to 25 parts by weight of foamed polyethylene particles, 1 to 10 parts by weight of a PHA resin, 3 to 20 parts by weight of a water-soluble adhesive (methyl cellulose), 10 to 20 parts by weight of a moisturizer, 2 to 5 parts by weight of a drying agent 60 to 65 parts by weight of a filler and 4 to 7 parts by weight of a thickener were added as a second additional component to 100 parts by weight of the first addition of the first additional component, 24 to 25 parts by weight of carbon fibers, 7 to 10 parts by weight of a flame retardant, 8 to 13 parts by weight of an ultraviolet screening agent and 2 to 3 parts by weight of a surface protective agent are blended and finally 30 to 40 parts by weight A can be formed by the addition of distilled water.
도 1은 본 발명의 실시예에 따른 피니싱 호일 접착용 친환경 접착제 조성물의 전체적인 제조 과정을 나타내는 흐름도이다. 도 2는 도 1의 피니싱 호일 접착용 친환경 접착제 조성물의 전체적인 제조 과정 중 단계(S10)의 접착제 조성물 제조 과정(S10)을 나타내는 흐름도이다. BRIEF DESCRIPTION OF THE DRAWINGS FIG. 1 is a flow chart showing the overall manufacturing process of an environmentally friendly adhesive composition for bonding a finishing foil according to an embodiment of the present invention. FIG. FIG. 2 is a flowchart showing an adhesive composition manufacturing process (S10) in step S10 in the entire manufacturing process of the environmentally friendly adhesive composition for bonding the finishing foil of FIG.
도 1을 참조하면, 접착제 조성물 제조 과정(S10), 대상에 도포하는 과정(S20), 피니싱 호일 접합 과정(S30), 열간프레스(Hot press) 과정(S40)을 포함할 수 있다.Referring to FIG. 1, an adhesive composition manufacturing process (S10), a coating process (S20), a finishing foil bonding process (S30), and a hot press process (S40) may be included.
먼저, 도 2를 참조하여 단계(S10)의 접착제 조성물 제조 과정에 대해서 살펴보면, PVAc(Polyvinyl Acetate), PAV(Polyvinyl Alcohol), PLA(PolyLactic Acid)를 1 : 0.8 내지 0.9 : 0.2 내지 0.3의 중량비로 준비한다(S11).Referring to FIG. 2, the adhesive composition of step S10 is prepared by mixing polyvinyl acetate (PVAc), polyvinyl alcohol (PAV) and polylactic acid (PLA) at a weight ratio of 1: 0.8 to 0.9: 0.2 to 0.3 (S11).
여기서, PVAc와 PLA의 혼합액 표면에 PVA가 일반적인 혼합 또는 자연분해 캡슐형으로 준비될 수 있으며, 자연분해 캡슐형으로 형성된 캡슐에는 희석제가 포함됨으로써, PVA는 반드시 PVAc 및 PLA 혼합액의 표면 전체에 균등하게 분포해야 하는 것은 아니고, 경우에 따라서는 국부적으로 캡슐형 PVA가 혼합되지 않는 부위가 존재할 수도 있다. 다만, PVA는 PVAc 및 PLA 혼합액의 표면 전체 면적에서 60% 이상에 분포되는 것이 바람직할 수 있다. Here, the PVA can be prepared as a general mixed or naturally decomposed capsule type on the surface of the mixed solution of PVAc and PLA, and the capsule formed as a natural decomposition capsule type contains a diluent, so that the PVA must be uniformly distributed over the entire surface of the mixed solution of PVAc and PLA It is not necessarily distributed, and in some cases, there may be a site where the encapsulated PVA is not mixed locally. However, PVA may preferably be distributed in an amount of 60% or more of the entire surface area of the mixed solution of PVAc and PLA.
여기 사용되는 캡슐이 분해시 사용되는 희석제는 PVAc 및 PLA 혼합액에 PVA에 의한 수지의 점도를 감소시키기 위하여 전형적으로 사용되는 것을 사용하거나, 본 발명의 일 실시예로, 스티렌 또는 크리프(creep)에 악영향이 없이 구조 접착제의 작용 시간을 연장하도록, 구조 접착제용으로 유용한 폴리머 반응성 희석제로서 기능이 있는, 저분자량, 폴리머 수반응성(moisture reactive) 조성물을 활용할 수 있다.The diluent used in the dissolution of the capsules used herein may be one which is typically used to reduce the viscosity of the PVA-based resin in the PVAc and PLA mixed solution, or in one embodiment of the present invention, styrene or creep may be adversely affected A low molecular weight, polymeric water reactive composition capable of functioning as a polymer reactive diluent useful for structural adhesives can be utilized to prolong the duration of action of the structural adhesive without the use of a polymeric reactive diluent.
즉, 희석제는 PVAc(Polyvinyl Acetate), PAV(Polyvinyl Alcohol), PLA(PolyLactic Acid) 총량을 기준으로 5 내지 6 중량% 사이에서 폴리머 반응성 희석제를 활용함으로써, 단계(S12)의 혼합물 생성을 위한 작용 시간을 연장하는 효과를 제공할 수 있다. That is, the diluent may be added to the active time for the production of the mixture of step S12 by utilizing a polymer reactive diluent between 5 and 6 wt% based on the total amount of PVAc (Polyvinyl Acetate), PAV (Polyvinyl Alcohol), PLA (Polylactic Acid) Can be provided.
본 발명에서, PVA의 함량이 너무 적으면 소망하는 결합력을 발휘할 수 없고, 반대로 너무 많으면 상대적으로 PVAc 및 PLA의 함량이 줄어들어 부피 변화로 인한 응력을 해소할 수 없고 접착성이 저하될 수 있다. 반대로, PVAc, PLA의 함량이 상기 중량비에 비해 과소해지면 접착제의 연신율이 불충분할 수 있으며, PVAc, PLA 함량이 상기 중량비에 비해 과대해지면 높은 친화성으로 인해 접착제의 대상에서의 분리를 유발할 수 있다. 따라서, 부착되는 대상의 종류 등을 고려하여 PVAc(Polyvinyl Acetate), PAV(Polyvinyl Alcohol), PLA(PolyLactic Acid), 그리고 도포 대상 간에 우수한 결합력을 나타낼 수 있고, 연신율에 의한 응력 해소의 효과를 발휘할 수 있도록 PVAc, PAV, PLA를 1 : 0.8 내지 0.9 : 0.2 내지 0.3의 중량비로 준비하는 것이다. In the present invention, when the content of PVA is too small, the desired binding force can not be exerted. On the other hand, when the content is too large, the content of PVAc and PLA is relatively decreased, stress due to volume change can not be eliminated and adhesiveness may be deteriorated. On the other hand, if the content of PVAc and PLA is less than the above-mentioned weight ratio, the elongation of the adhesive may be insufficient, and if the content of PVAc and PLA is excessively larger than the above-mentioned weight ratio, separation of the adhesive from the object may be caused due to high affinity. Therefore, it is possible to exhibit excellent bonding force between PVAc (Polyvinyl Acetate), PAV (Polyvinyl Alcohol), PLA (Polylactic Acid) and the object to be coated in consideration of the kind of object to be attached, PVAc, PAV, and PLA in a weight ratio of 1: 0.8 to 0.9: 0.2 to 0.3.
본 발명의 다른 실시예로, 부피팽창이 기준치 이상 발생 가능한 피니싱 호일의 경우에는 연신율이 우수한 PVAc 및 PLA의 함량을 상대적으로 증가시킬 수 있고, 반대로, 부피 팽창보다는 접착력의 강화가 필요한 피니싱 호일의 경우에는 상대적으로 PVA의 함량이나 두께를 증가시킬 수 있다.According to another embodiment of the present invention, in the case of a finishing foil in which volume expansion can occur above a reference value, the content of PVAc and PLA having an excellent elongation can be relatively increased. On the contrary, in the case of a finishing foil It is possible to increase the content and thickness of PVA relatively.
한편, 본 발명에 사용되는 PLA는 친환경적인 폴리머(polymer) 역할을 수행하기 위해 준비되며, 재생 가능한 옥수수 등 식물을 발효시켜 얻은 락타이드 또는 락트산을 중합하여 제조된 열가소성 폴리에스테르로서 화석 자원 고갈에 무관할 뿐만 아니라 사용 후 매립 등 방식으로 쉽게 분해할 수 있는 친환경적인 특성이 있다.Meanwhile, the PLA used in the present invention is a thermoplastic polyester prepared by polymerizing lactide or lactic acid obtained by fermenting plants such as renewable corn, which is prepared to perform an eco-friendly polymer and is free of fossil resource depletion There is also an eco-friendly characteristic that can be easily disassembled by reclamation after use.
PLA는 락트산 또는 락타이드를 중합시켜 제조할 수 있으며, 필요에 따라서는, 에틸렌글리콜 또는 프로필렌글리콜 등의 글리콜화합물, 에탄디오산(ethanedioic acid) 또는 테레프탈산 등의 디카복실산, 글리콜산 또는 2-히드록시벤조산 등의 히드록시카르본산 또는 카프로락톤 또는 프로피오락톤 등의 락톤류와 같은 적절한 단량체와 공중합될 수도 있다. 그리고, PLA는 통상적으로 D,L-PLA, meso-PLA, D-PLA, L-PLA 등으로 구분될 수 있는데, 본 발명에서는 그 종류에 제한되지 않고, 상술한 PLA를 단독으로 혹은 2종 이상 혼합하여 이용할 수 있다.PLA can be prepared by polymerizing lactic acid or lactide, and if necessary, a glycol compound such as ethylene glycol or propylene glycol, a dicarboxylic acid such as ethanedioic acid or terephthalic acid, glycolic acid or 2-hydroxy Hydroxycarboxylic acids such as benzoic acid or lactones such as caprolactone or propiolactone. The PLA may be classified into D, L-PLA, meso-PLA, D-PLA, L-PLA and the like in the present invention. Can be mixed and used.
단계(S11) 이후, PVAc, PAV, PLA 혼합물 전체 중량인 100 중량부에 대해서 발포타입 폴리에틸렌 입자를 20 내지 25 중량부, PHA(Poly Hydroxyl Alkanoate) 수지 1 내지 10 중량부, 수용성 접착제(methyl cellulose) 3 내지 20 중량부, 보습제(glcerine) 10 내지 20 중량부, 에스테르(drying agent) 2 내지 5 중량부의 비율로 교반하여 제 1 혼합물을 생성한다(S12).After step S11, 20 to 25 parts by weight of foamed polyethylene particles, 1 to 10 parts by weight of PHA (polyhydroxylalkanoate) resin, 1 to 10 parts by weight of water-soluble adhesive (methyl cellulose) are added to 100 parts by weight of PVAc, PAV, 3 to 20 parts by weight, 10 to 20 parts by weight of a moisturizing agent (glcerine) and 2 to 5 parts by weight of a drying agent (S12).
발포타입 폴리에틸렌 입자는 폴리에틸렌 원료를 사용하며, 발포제와 함께 스크류 방식에 의한 발포타입 폴리에틸렌에 대한 배합을 수행한 뒤, 고체 형태로 형성하여 미립자로 분쇄하여 형성될 수 있다. 최종 제조되는 피니싱 호일 접착용 친환경 접착제 조성물가 부착 대상에 접착되어 건조시 인장강도 향상을 위해 폴리에틸렌의 중량평균 분자량은 130,000g/mol 이상, 용융지수는 0.3 내지 7g/12분(150℃)인 것이 바람직하며, 발포타입 폴리에틸렌은 상술한 바와 같이 용융지수가 용융지수는 0.3 내지 7g/12분이고, 그 밖에 분자량분포(PI)가 5.7 이상이며, 용융강도가 35 mN 이상인 폴리에틸렌 기반 원료 100 중량부에 대하여 발포제 12 내지 23 중량부를 배합한다. The foamed polyethylene particles may be formed by using a raw material of polyethylene and blending with foaming type polyethylene by a screw method together with a foaming agent, and then forming the foamed polyethylene into a solid form and pulverizing it into fine particles. Eco-friendly adhesive composition for bonding a finishing foil to be finally prepared has a weight average molecular weight of polyethylene of 130,000 g / mol or more and a melt index of 0.3 to 7 g / 12 min (150 DEG C) for adhesion to an object to be attached and improving tensile strength upon drying The foamed polyethylene preferably has a melt index of 0.3 to 7 g / 12 min, a melt index of 5.7 or more, and a melt index of 35 mN or more, based on 100 parts by weight of the polyethylene- And 12 to 23 parts by weight of a foaming agent.
발포타입 폴리에틸렌을 제조하기 위해 사용되는 발포제의 함량이 23 중량부를 초과하면 강성과 내열성, 표면 경도가 현저히 저하되어 절연제의 응용에 부적합하므로 바람직하지 않으며, 12 중량부 미만이면 비중, 발포성, 성형성, 충격특성이 저하되어 바람직하지 않다. 이때 주로 사용되는 화학 발포제는 Sodium bicarbonate(NaHCO3)가 주로 사용되는 것이 바람직하다.When the content of the blowing agent used for producing the foamed polyethylene is more than 23 parts by weight, rigidity, heat resistance and surface hardness are significantly lowered, which is not preferable because it is unsuitable for the application of an insulating material. When the content is less than 12 parts by weight, , The impact characteristics are deteriorated and it is not preferable. It is preferable that sodium bicarbonate (NaHCO 3 ) is mainly used as a chemical foaming agent mainly used.
본 발명의 다른 실시예로, 발포타입 폴리에틸렌 혼합물을 제조하기 위한 폴리에틸렌은 단독으로 사용하거나 폴리에틸렌 혼합물로 형성된 뒤 발포과정을 거쳐 사용될 수 있다. 여기서, 폴리에틸렌 혼합물은 폴리에틸렌 100 중량부에 대해서 에틸렌비닐초산 코폴리머(EVA) 25 내지 30 중량부, 폴리우레탄 10 내지 15 중량부로 구성되는 수지조성물을 활용할 수 있으며, 이상과 같은 수지조성물에 의해 제조되는 합성수지 소재는 폴리에틸렌만을 사용한 수지에 의해 인장강도, 굴곡강도, 하중변형온도, 아이죠드 충격강도에서 향상된 성능을 나타낼 뿐만 아니라, 조성 재료 자체가 저렴하여 제조하는 원가를 낮출 수 있다. In another embodiment of the present invention, the polyethylene for preparing the foamed polyethylene mixture may be used alone or may be used after a foaming process which is formed of a polyethylene mixture. Here, the polyethylene mixture may be a resin composition comprising 25 to 30 parts by weight of an ethylene vinyl acetate copolymer (EVA) and 10 to 15 parts by weight of a polyurethane with respect to 100 parts by weight of polyethylene, The synthetic resin material exhibits improved performance in terms of tensile strength, flexural strength, load deformation temperature and Izod impact strength due to the resin using only polyethylene, and the cost of the manufacturing can be reduced because the composition material itself is inexpensive.
PHA 수지는 여러 가지 탄소곁사슬이 있는 히드록시산 폴리에스테르의 총칭이다. PHA 수지는 과립막 내의 중합효소에 의한 D(-)-3-히드록시지방산 CoA의 중합에 의해 생성되지만 최근 어떤 종류의 세균에서는 여러 가지 길이의 곁사슬이 있는 히드록시산의 중합체, 혹은 3-히드록시부티르산과의 공중합체인 PHA가 발견되고 있다. 혼합수지 중 PHA 수지는 Poly Hydroxyl Alkanoate의 약자로써, 여러 가지 탄소곁사슬이 있는 히드록시산 폴리에스테르의 총칭이다. PHA 수지는 과립막 내의 중합효소에 의한 D(-)-3-히드록시지방산 CoA의 중합에 의해 생성되지만 최근 어떤 종류의 세균에서는 여러 가지 길이의 곁사슬이 있는 히드록시산의 중합체, 혹은 3-히드록시부티르산과의 공중합체인 PHA가 발견되고 있다. 이러한 PHA 수지를 PVAc, PAV, PLA 혼합물에 혼합하게 되면, PLA 기반 원료에 유연성을 부여할 수 있는 효과를 제공하여 최종 접착제로서 유도성을 부여할 수 있다. PHA resin is a generic name of hydroxy acid polyester having various carbon side chains. PHA resin is produced by the polymerization of D (-) - 3-hydroxy fatty acid CoA by a polymerase in the granular membrane, but recently, in some bacteria, a polymer of hydroxy acid having side chains of various lengths, PHA is found as a copolymer with roxybutyrate. The PHA resin in the mixed resin is an abbreviation of Poly Hydroxyl Alkanoate. It is a generic name of hydroxy acid polyester having various carbon side chains. PHA resin is produced by the polymerization of D (-) - 3-hydroxy fatty acid CoA by a polymerase in the granular membrane, but recently, in some bacteria, a polymer of hydroxy acid having side chains of various lengths, PHA is found as a copolymer with roxybutyrate. When such a PHA resin is mixed with the PVAc, PAV, and PLA mixture, flexibility can be imparted to the PLA-based raw material, thereby providing inductive properties as a final adhesive.
단계(S12)에서 PVAc, PAV, PLA 혼합물에 발포타입 폴리에틸렌 입자, PHA 수지를 혼합한 상태에서, 수용성 접착제(methyl cellulose)를 정량 함께 혼합기에서 교반하면서, 보습제(glcerine)를 첨가하면서 혼합기 온도를 30 내지 35℃의 온도로 설정하여 30분 정도 교반을 유지한 뒤, 중합 완료 전에 에스테르(drying agent)를 혼합한다. 여기서 PVAc, PAV, PLA 혼합물 전체 중량인 100 중량부에 대해서 에스테르(drying agent)를 2 중량부가 미달인 경우 최종 생성되는 피니싱 호일 접착용 친환경 접착제의 고형화가 진행되지 않으며, 반대로 5 중량부를 초과하는 경우 단계(S13)에서 단계(S15)를 진행하는 과정에서 고형화가 현저히 진행되는 문제점이 발생할 수 있다.In step S12, while mixing the PVAc, PAV, and PLA mixture with the foamed polyethylene particles and the PHA resin, while stirring the water-soluble adhesive (methyl cellulose) in a mixer while adding the glcerine, To 35 캜 and stirring is maintained for about 30 minutes, followed by mixing with a drying agent before completion of the polymerization. If the amount of the drying agent is less than 2 parts by weight based on 100 parts by weight of the PVAc, PAV and PLA mixture, the final eco-friendly adhesive for bonding the finishing foil is not solidified. On the other hand, There may occur a problem that the solidification progresses significantly in the course of proceeding from the step S13 to the step S15.
본 발명에서 사용되는 에스테르는 oleic acid와 stearic acid를 1 : 0.5 내지 1의 비율로 혼합하여 사용할 수 있다. The ester used in the present invention may be a mixture of oleic acid and stearic acid in a ratio of 1: 0.5 to 1.
단계(S12) 이후, 제 1 혼합물 100 중량부에 대해서 충진제 60 내지 65 중량부, 증점제 4 내지 7 중량부를 배합하여 교반하여 제 2 혼합물을 생성한다(S13). 보다 구체적으로, 단계(S12)에서 생성된 제 1 혼합물인 PVAc(Polyvinyl Acetate), PAV(Polyvinyl Alcohol), PLA(PolyLactic Acid), 발포타입 폴리에틸렌 입자, PHA(Poly Hydroxyl Alkanoate) 수지, 수용성 접착제(methyl cellulose), 보습제(glcerine), 에스테르(drying agent)의 혼합물에 충진제 및 증점제를 추가한다.After step S12, 60 to 65 parts by weight of a filler and 4 to 7 parts by weight of a thickener are added to 100 parts by weight of the first mixture and stirred to produce a second mixture (S13). More specifically, the first mixture produced in step S12, such as PVAc (Polyvinyl Acetate), PAV (Polyvinyl Alcohol), PLA (Polylactic Acid), foamed polyethylene particles, PHA (polyhydroxylalkanoate) Add a filler and thickener to a mixture of cellulose, glcerine, and drying agent.
단계(S13)에서 사용되는 충진제는 탄산칼슘, 탈크, 클레이, 실리카, 산성백토를 포함하는 그룹에서 선택되는 하나 이상인 것을 특징으로 한다. The filler used in step S13 is at least one selected from the group consisting of calcium carbonate, talc, clay, silica and acidic clay.
본 발명의 일 실시예로, 탈크를 이용시 접착제의 성형성과 내가수분해성능을 향상시키기 위하여 첨가되는 것으로, 1액형 접착제 조성물을 구성하는 원재료인 제 1 혼합물 100 중량부에 대하여 충진제 60 내지 65 중량부를 사용할 수 있다. 여기서, 탈크가 60 중량부 미만일 경우 치수안정성 개선효과가 떨어지며, 65 중량부를 초과하였을 경우 접착제로 사용하여 경화시 내구 및 내열성이 현저하게 저하되는 우려가 발생할 수 있다. In an embodiment of the present invention, 60 to 65 parts by weight of a filler is added to 100 parts by weight of the first mixture, which is a raw material of the one-pack type adhesive composition, in order to improve the moldability of the adhesive and the moisture- Can be used. If the amount of the talc is less than 60 parts by weight, the effect of improving dimensional stability is deteriorated. If the amount of the talc is more than 65 parts by weight, there is a possibility that the durability and heat resistance are significantly lowered when cured.
그리고 최종 생산되는 피니싱 호일 접착용 친환경 접착제 조성물 용액의 점도를 증가시키기 위한 증점제는 실리카, 흄실리카, 벤토나이트, 클레이, 아마이드, 셀룰로오스로 구성된 그룹에서 선택되는 어느 하나 또는 2종 이상 혼합한 것을 사용하며, 제 1 혼합물 100 중량부에 증점제 4 중량부 미만인 경우, 최종 생산된 접착제 조성물이 피니싱 호일로부터 흘러내릴 수 있으며, 반대로 7 중량부를 초과하는 경우 피니싱 호일과 접착제 조성물이 접하는 경우 경화가 너무 빨리 진행할 수 있다. The thickener for increasing the viscosity of the eco-friendly adhesive composition solution for final bonding of finishing foil is selected from the group consisting of silica, fumed silica, bentonite, clay, amide and cellulose, If the amount of the thickener is less than 4 parts by weight in the first mixture 100 parts by weight, the finally produced adhesive composition may flow down from the finishing foil. On the other hand, if the amount exceeds 7 parts by weight, .
단계(S13) 이후, 첨가제로 제 2 혼합물 100 중량부에 대해서 탄소 섬유 24 내지 25 중량부, 난연제 7 내지 10 중량부, 자외선차단제 8 내지 13 중량부, 표면보호제 2 내지 3 중량부를 배합한다(S14). After step S13, 24 to 25 parts by weight of carbon fibers, 7 to 10 parts by weight of a flame retardant, 8 to 13 parts by weight of an ultraviolet screening agent and 2 to 3 parts by weight of a surface protective agent are added to 100 parts by weight of the second mixture as an additive (S14 ).
탄소 섬유에 대해서 살펴보면, 탄소 섬유는 피니싱 호일과 접착제 조성물 간의 전도성의 필요에 따라 용량이 조절될 수 있으며, 1액형 피니싱 호일 접착용 친환경 접착제 조성물은 탄소 섬유를 첨가 혼합하여 탄소 섬유 강화형(CFR, Garbon Fiber Reinforced Plastic)에 해당하는 레진을 수득하게 되는데, 탄소 섬유 강화 1액형 피니싱 호일 접착용 친환경 접착제 조성물에 포함되는 탄소 섬유는 철보다 강하고 알루미늄보다 가벼우며 가공성이 우수하다는 장점을 제공할 수 있다. 즉, 1액형 피니싱 호일 접착용 친환경 접착제 조성물의 경화시 인장 강도가 상대적으로 우수한 PVAc, PAV, PLA 혼합물에 파단 강도가 우수한 탄소 섬유를 첨가 혼합하여 접착제로서 요구되는 파단강도를 갖추게 되고, PVAc, PAV, PLA 혼합물에 난연성을 부가하여 접착 대상에서 발생할 수 있는 화재 등에 난연성을 갖추게 함으로써, 가격 경쟁력이 높으면서도 난연성 등과 같은 기능성을 발휘할 수 있다. As for the carbon fiber, the carbon fiber can be adjusted in its capacity depending on the need for conductivity between the finishing foil and the adhesive composition. The eco-friendly adhesive composition for bonding one-pack type finishing foil is prepared by adding carbon fibers to the carbon fiber- Garbon Fiber Reinforced Plastic). The carbon fiber contained in the eco-friendly adhesive composition for bonding the carbon fiber-reinforced one-part finishing foil has the advantage that it is stronger than iron, lighter than aluminum, and excellent in workability. That is, the carbon fiber having excellent fracture strength is added to the mixture of PVAc, PAV and PLA having relatively good tensile strength at the time of curing of the environmentally friendly adhesive composition for bonding one-pack type finishing foil, By adding flame retardancy to the PLA mixture and providing flame retardancy to a fire or the like which may occur in an object to be bonded, functionality such as flame retardancy and the like with high price competitiveness can be exhibited.
다음으로, 난연제에 대해서 살펴보면, 난연제는 몰리브덴산 안티몬, 산화몰리브덴, 수산화마그네슘, 수산화알미늄 중 어느 하나 또는 2종 이상 혼합한 것을 사용한다. 특히 수산화알미늄(Al(OH)3)은 경화된 액형 피니싱 호일 접착용 친환경 접착제 조성물에 열이 가해져서 500℃ 이상이 되면 미세 다공질이 무수히 많은 활성알루미나로 변화되어 흡착 성능을 가지게 되므로 연소시 발생하는 다이옥신, 염화수소가스(HCl) 등 유해 물질을 흡착하며 열 분해시 흡열 반응을 하여 냉각 효과도 있고 불연성으로서 내수, 내산성이 우수하다. 또한 상기 난연제들을 병용 사용하여 난연 효과의 향상을 기대할 수 있다.Next, regarding the flame retardant, the flame retardant is one selected from the group consisting of antimony molybdate, molybdenum oxide, magnesium hydroxide, and aluminum hydroxide or a mixture of two or more thereof. Particularly, aluminum hydroxide (Al (OH) 3 ) is heat-applied to an environmentally-friendly adhesive composition for adhering a cured liquid type finishing foil and when the temperature exceeds 500 ° C., micropores are changed into a large number of active alumina, Dioxins, HCl (HCl), and it absorbs harmful substances such as HCl. It absorbs heat during thermal decomposition and has a cooling effect. It is nonflammable and has excellent water resistance and acid resistance. In addition, the flame retardant effect can be expected to be improved by using the above flame retardants in combination.
다음으로, 자외선차단제는 폴리에틸렌 수지 또는 수성아크릴계 합성수지 100 중량부에 대해서 100 내지 1000㎛의 분체의 평균입도를 갖는 이산화티탄(TiO2) 34 내지 37 중량부와 산화아연(ZnO2) 33 내지 35 중량부를 혼합한 뒤, 혼합물에 감마아미노에틸렌아미노프로필트리메톡시실란의 실란계 화합물 25 내지 27 중량부를 혼합하여 점착성을 부여하고, 혼합 용액에 pH 5 내지 7의 실리콘 오일 2 내지 5 중량부, 계면활성제 2 내지 5 중량부를 혼입하여 15℃ 내지 25℃에서 30분간 교반하여 표면을 개질하여 자외선차단제를 생성할 수 있다. 이때, 이산화티탄(TiO2)의 평입도가 100㎛ 이하면 UV-B(290-320nm)의 영역이 효과적으로 차단되며, 이산화티탄(TiO2)의 평입도가 1000㎛ 이상이면 UV-B(290-320nm)의 영역이 효과적으로 차단될 수 있다. 또한, 실리콘 오일이 pH 5 이하의 산성인 경우에는 자외선 차단제의 점착성이 떨어지는 문제가 발생할 수 있다.Next, 34 to 37 parts by weight of titanium dioxide (TiO 2 ) having an average particle size of 100 to 1000 μm as a powder of 100 parts by weight of polyethylene resin or aqueous acrylic synthetic resin, 33 to 35 parts by weight of zinc oxide (ZnO 2 ) And 25 to 27 parts by weight of a silane compound of gamma aminoethylaminopropyltrimethoxysilane are mixed to give a tackiness. To the mixture is added 2 to 5 parts by weight of a silicone oil having a pH of 5 to 7, a surfactant 2 to 5 parts by weight are mixed and stirred at 15 ° C to 25 ° C for 30 minutes to modify the surface to produce an ultraviolet screening agent. At this time, if the flatness degree of titanium dioxide (TiO 2 ) is 100 μm or less, the region of UV-B (290-320 nm) is effectively blocked. If the flatness of titanium dioxide (TiO 2 ) -320 nm) can be effectively blocked. In addition, when the silicone oil is acidic at pH 5 or less, the problem of poor adhesion of the ultraviolet screening agent may occur.
표면보호제는 무기고분자 소재를 포함하고 있으므로 접착 강도가 우수하고 내수성이 강하므로, 습윤 상태에서도 1액형 피니싱 호일 접착용 친환경 접착제 조성물이 도포될 수 있도록 하며 수중침지에 의하여 박리 또는 박락되지 않도록 하는 역할을 수행한다. 또한, 표면보호제는 자외선에 의하여 변색되지 않으므로 직사광선에 많이 노출되는 교량, 교각, 항만, 운동장 등의 콘크리트 구조물의 건설에 사용되기 적합하며, 경화 후에 불연성 재질로 변하므로 화재 발생시 열기에 의하여 쉽게 손상되지 않는다는 장점도 있으며, 표면보호제는 1액형 도료이므로, 별도의 경화제를 사용하지 않고 쉽게 경화될 수 있어서, 사용이 편리하고 인체에 유해하지 않다는 장점도 제공할 수 있다.Since the surface protective agent contains an inorganic polymer material, it has an excellent adhesive strength and a high water resistance, so that it can be coated with an eco-friendly adhesive composition for bonding a one-part finishing foil even in a wet state and does not peel off or peel off by immersion in water . In addition, since the surface protective agent is not discolored by ultraviolet rays, it is suitable for use in construction of concrete structures such as bridges, bridges, harbors, and playgrounds that are exposed to direct sunlight and is changed into incombustible material after curing. Since the surface protective agent is a one-pack type paint, it can be easily cured without using a separate curing agent, which is advantageous in that it is easy to use and is not harmful to human body.
단계(S14) 이후, 배합물 100 중량부에 대해서 30 내지 40 중량부의 증류수를 첨가하고, 100 내지 150℃의 온도에서 1 시간 내지 2 시간 사이에서 가열 및 교반한다(S15).After step S14, 30 to 40 parts by weight of distilled water is added to 100 parts by weight of the blend, and the mixture is heated and stirred at a temperature of 100 to 150 DEG C for 1 to 2 hours (S15).
단계(S14) 이후, 가열 및 교반 완료된 조성물에 대해서 진공탈포하여 접착제 조성물 생성을 완료한다(S16). After the step S14, the heated and stirred composition is vacuum-defoamed to complete the formation of the adhesive composition (S16).
한편, 단계(S11) 내지 단계(S16)를 포함하는 단계(S10) 이후의 단계(S20) 내지 단계(S40)에 대해서 살펴보도록 한다. Meanwhile, steps S20 to S40 after the step S10 including the steps S11 to S16 will be described.
즉, 단계(S10)에 따라 생성된 피니싱 호일 접착용 친환경 접착제 조성물을 단계(S20)에서는 피니싱 호일이 부착되는 대상에 도포하는데, 본 발명의 다른 실시예로, 단계(S10)에서 기술된 접착제를 제조하는 단계에서의 접착제는 핫멜트(Hot melt) 방식의 접착제로 구성하는 것이 공정적 측면에서나 제조원가 측면에서 바람직할 수 있다. That is, the environmentally friendly adhesive composition for bonding the finishing foil produced according to step S10 is applied to the object to which the finishing foil is attached in step S20. In another embodiment of the present invention, the adhesive described in step S10 The adhesive in the manufacturing step may be preferably composed of a hot melt type adhesive in terms of process and manufacturing cost.
이에 따라 피니싱 호일 접착용 친환경 접착제 조성물은 이종의 부착 대상에 피니싱 호일(합성 수지 필름 및 피니싱 종이 호일 등)에 대한 접착력이 확보되어야 하며, 추가로 도포 전 부착 대상과 피니싱 호일 간에 기계적인 맞물림을 사전 형성할 수 있다. 어떠한 계면을 미시적인 측면에서 관찰했을 때에, 그 계면은 고르지 못하고 돌기나 홈, 스크래치 등의 표면 상태를 가진다. 이러한 계면에 액상의 피니싱 호일 접착용 친환경 접착제 조성물가 계면의 돌기들 사이나 홈과 같은 곳에 스며들게 되고 경화 또는 고화가 된다. 단단하게 경화 또는 고화된 피니싱 호일 접착용 친환경 접착제 조성물은 기계적으로 맞물려 있어 마치 땅에 말뚝을 박은 것이나 바다에 닻이 걸려있는 것과 같은 효과를 지니게 된다.Accordingly, the eco-friendly adhesive composition for bonding the finishing foil must secure adhesion to the finishing foil (such as a synthetic resin film and a finishing paper foil) to different kinds of objects to be adhered, and further, a mechanical engagement between the object to be adhered and the finishing foil . When any interface is observed from the microscopic side, the interface is uneven and has surface states such as projections, grooves, and scratches. At this interface, the environmentally friendly adhesive composition for bonding the liquid finishing foil is impregnated and hardened or solidified, such as protrusions or grooves at the interface. The eco-friendly adhesive composition for bonding a hardened or solidified finishing foil is mechanically engaged and has the same effect as if a pile was placed on the ground or an anchor was caught in the sea.
기계적 맞물림을 앵커링(Anchoring) 이라고 하며 이러한 기계적인 맞물림에 의해 피니싱 호일 접착용 친환경 접착제 조성물과, 피니싱 호일 및 부착 대상 간에는 접착력을 강력하게 형성할 수 있다. The mechanical engagement is referred to as anchoring, and by such mechanical engagement, it is possible to strongly form an adhesive force between the environmentally friendly adhesive composition for bonding the finishing foil, the finishing foil and the object to be adhered.
이와 같이, 우수한 접착력 확보를 위해서 피니싱 호일 및 부착 대상 간의 접착 면에는 에칭(Etching), 코로나 (Corona)처리 등의 표면처리를 하는 것이 바람직하다.As described above, it is preferable to perform surface treatment such as etching or corona treatment on the adhesion surface between the finishing foil and the object to be adhered in order to secure an excellent adhesion.
그리고 앵커링(Anchoring) 만으로는 접착력 형성과 그 원리를 다 수용할 수가 없기 때문에 피니싱 호일 접착용 친환경 접착제 조성물가 부착되는 부착 대상 소재에 따라 피니싱 호일 접착용 친환경 접착제 조성물의 그 소재와 원리를 고려해야 한다.Since the anchoring alone can not accommodate the adhesive force and its principle, the material and principle of the eco-friendly adhesive composition for bonding the finishing foil should be considered according to the material to which the eco-friendly adhesive composition for adhering the finishing foil adheres.
즉, 피니싱 호일과 피니싱 호일 접착용 친환경 접착제 조성물 사이에는 고분자 사이의 접착원리를 고려해야 한다. 단순히 기계적인 맞물림의 효과뿐이 아니라 고분자 계면 사이에서의 접착은 열역학적으로 서로 상용성(Compatibility)이 있거나 부분적으로 상용성(Compatibility)을 지니게 되면, 계면과 계면 사이에서 고분자 사슬의 확산 효과에 의해서 상호 확산된 고분자 사슬이 다른 고분자 사슬과 엉킴(entanglement)을 형성하게 된다.That is, between the finishing foil and the environmentally friendly adhesive composition for bonding the finishing foil, the bonding principle between the polymers must be considered. Not only the mechanical merge effect but also the adhesion between the polymer interfaces can be thermodynamically compatible or partially compatible with each other due to the diffusion effect of the polymer chain between the interface and the interface The diffused polymer chains form entanglement with other polymer chains.
이후 외력에 의해서 두 계면을 분리할 때에 고분자 사슬의 엉킴(entanglement)이 풀리거나 고분자 사슬이 파괴되게 되는데 이러한 것이 접착력 형성의 요인이 된다.When the two interfaces are separated by an external force, the entanglement of the polymer chain is loosened or the polymer chain is destroyed, which is a factor of forming the adhesion force.
그리고 단계(S20)에서 피니싱 호일이 부착되는 대상에 피니싱 호일 접착용 친환경 접착제 조성물을 도포하는 방법은 크게 액형과 고형의 접착제를 사용하는 두 가지 분류로 나눌 수 있다. 액형의 피니싱 호일 접착용 친환경 접착제 조성물을 도포하는 방법은 스프레이(Spray)나 바코팅(Bar Coating)과 같은 방법으로 할 수 있으며, 고형의 접착제의 경우에는 일반적으로 가열기구를 이용하여 녹여서 붙일 수가 있는데 상기 고형의 접착제는 필름 형태로 제조된 것을 이용하여 열압착(thermal lamination) 방법으로 접착하는 것이 바람직하다.The method of applying the environmentally friendly adhesive composition for bonding the finishing foil to the object to which the finishing foil is attached in step S20 can be roughly divided into two types, that is, a liquid type and a solid type adhesive. The method of applying the environmentally friendly adhesive composition for bonding the liquid type finishing foil can be performed by a method such as spraying or bar coating. In the case of a solid type adhesive, the adhesive can be usually melted using a heating mechanism It is preferable that the solid adhesive is adhered by a thermal lamination method using a product made in the form of a film.
단계(S20) 이후, 피니싱 호일 접합 과정(S30)을 거쳐 열간프레스(Hot press) 과정(S40)을 수행하는데, 즉, 피니싱 호일을 접착제가 도포된 부착 대상으로의 접합 과정과 동시에 또는 이후에 열간프레스(Hot press)로 100 ℃이하로 가열, 압착시키며, 이때의 온도 또한 100℃를 초과 시 PVAc, PLA, PVA 혼합물에 의해 피니싱 호일이 변형될 수 있다.After the step S20, the hot press process S40 is performed through the finishing foil joining process S30, that is, the finishing foil is heated at the same time as or after the bonding process to the object to which the adhesive is applied, When the temperature is also higher than 100 ° C, the finishing foil may be deformed by the mixture of PVAc, PLA and PVA.
1액형 피니싱 호일 접착용 친환경 접착제 조성물은 피니싱 호일의 평량이 30 이상 50g/m2 미만인 경우에는 양을 7 내지 12g/m2로, 피니싱 호일의 평량이 50 이상 70g/m2 미만인 경우에는 양을 10 내지 18g/m2, 피니싱 호일의 평량이 70 이상 100 이하인 경우 양을 17 내지 25m2으로 평량에 따라 접착제 조성물의 양을 가변하여 줄 수 있다. One-pack type finishing foil bonded friendly adhesive composition, if the basis weight of the finishing foil 30 at least 50g / m 2 is less than 7 to 12g / m 2 amount, the basis weight of the finishing foil, the amount, if more than 50 70g / m 2 is less than 10 to 18 g / m < 2 >, and the basis weight of the finishing foil is not less than 70 and not more than 100, the amount of the adhesive composition may be varied in the amount of 17 to 25 m < 2 >
이와 같이 구성되는 1액형 피니싱 호일 접착용 친환경 접착제 조성물은 실험결과, 내수성이 D2 등급이상이며, 내열성은 250℃까지 견디며, 내용제성이 우수하다. 또한 상온에서 적당한 경도(hardness)를 유지하고 수축, 팽창이 적고, 열압착 부착시 경도가 너무 높아 피니싱 호일이 변형되지 않으며, 장시간 사용 후에도 물성이 계속 유지됨을 알 수 있었다.As a result of the test, the eco-friendly adhesive composition for bonding a one-part finishing foil having the above structure has a water resistance of D 2 grade or higher, a heat resistance of 250 ° C, and excellent solvent resistance. Further, it was found that the hardness at room temperature was maintained, shrinkage and expansion were small, and the hardness was too high at the time of thermocompression bonding, so that the finishing foil was not deformed and the physical properties were maintained even after prolonged use.
한편, 하기의 표 1과 같이 기존의 피니싱 호일용 2액형 요소 멜라민계 제품이므로 친환경이 아니며, 2액형으로 사용 및 관리가 불편하다.On the other hand, as shown in Table 1 below, it is not environmentally friendly because it is a two-component urea melamine-based product for a conventional finishing foil.
그러나 본 발명에 따른 1액형 피니싱 호일 접착용 친환경 접착제 조성물은 친환경이며, 1액형 타입으로 현장 작업성도 편리하며, 초기 접착력 등의 물리적 특성도 우수하다. However, the eco-friendly adhesive composition for bonding the one-part finishing foil according to the present invention is eco-friendly, and is one-pack type, convenient in the field work, and has excellent physical properties such as initial adhesive strength.
추가로, 목가구용 피니싱 호일 접착에 1액형 피니싱 호일 접착용 친환경 접착제 조성물을 적용시 수성 친환경 생산 적용으로 작업 환경이 양호해 지며, 접착제의 2회 도포에서 1회 도포가 가능하므로 라인의 성력화 등이 가능하다. In addition, when applying the eco-friendly adhesive composition for bonding the one-part finishing foil to the finishing foil for wood furniture, the working environment is improved by applying the water-friendly eco-friendly production, and the application of the adhesive can be applied once twice. It is possible.
이상과 같이, 본 명세서와 도면에는 본 발명의 바람직한 실시예에 대하여 개시하였으며, 비록 특정 용어들이 사용되었으나, 이는 단지 본 발명의 기술 내용을 쉽게 설명하고 발명의 이해를 돕기 위한 일반적인 의미에서 사용된 것이지, 본 발명의 범위를 한정하고자 하는 것은 아니다. 여기에 개시된 실시예 외에도 본 발명의 기술적 사상에 바탕을 둔 다른 변형 예들이 실시 가능하다는 것은 본 발명이 속하는 기술 분야에서 통상의 지식을 가진 자에게 자명한 것이다.As described above, preferred embodiments of the present invention have been disclosed in the present specification and drawings, and although specific terms have been used, they have been used only in a general sense to easily describe the technical contents of the present invention and to facilitate understanding of the invention , And are not intended to limit the scope of the present invention. It is to be understood by those skilled in the art that other modifications based on the technical idea of the present invention are possible in addition to the embodiments disclosed herein.
Claims (2)
PVAc, PAV, PLA 혼합물 전체 중량인 100 중량부에 대해서 발포타입 폴리에틸렌 입자를 20 내지 25 중량부, PHA(Poly Hydroxyl Alkanoate) 수지 1 내지 10 중량부, 수용성 접착제(methyl cellulose) 3 내지 20 중량부, 보습제(glcerine) 10 내지 20 중량부, 에스테르(drying agent) 2 내지 5 중량부의 비율로 교반하여 제 1 혼합물을 생성하되, 발포타입 폴리에틸렌 입자는 폴리에틸렌 원료를 사용하며, 발포제와 함께 스크류 방식에 의한 발포타입 폴리에틸렌에 대한 배합을 수행한 뒤, 고체 형태로 형성하여 미립자로 분쇄하여 형성되며, 최종 제조되는 피니싱 호일 접착용 친환경 접착제 조성물가 부착 대상에 접착되어 건조시 인장강도 향상을 위해 폴리에틸렌의 중량평균 분자량은 130,000g/mol 이상, 용융지수는 0.3 내지 7g/12분(150℃)이고, 분자량분포(PI)가 5.7 이상이며, 용융강도가 35 mN 이상인 폴리에틸렌 기반 원료 100 중량부에 대하여 발포제 12 내지 23 중량부를 배합하며, 발포타입 폴리에틸렌 혼합물을 제조하기 위한 폴리에틸렌은 단독으로 사용하거나 폴리에틸렌 혼합물로 형성된 뒤 발포과정을 거쳐 사용되며, 폴리에틸렌 혼합물은 폴리에틸렌 100 중량부에 대해서 에틸렌비닐초산 코폴리머(EVA) 25 내지 30 중량부, 폴리우레탄 10 내지 15 중량부로 구성되는 수지조성물을 활용하며, PVAc, PAV, PLA 혼합물에 발포타입 폴리에틸렌 입자, PHA 수지를 혼합한 상태에서, 수용성 접착제(methyl cellulose)를 정량 함께 혼합기에서 교반하면서, 보습제(glcerine)를 첨가하면서 혼합기 온도를 30 내지 35℃의 온도로 설정하여 30분 정도 교반을 유지한 뒤, 중합 완료 전에 에스테르(drying agent)를 혼합하며, 에스테르는 oleic acid와 stearic acid를 1 : 0.5 내지 1의 비율로 혼합하여 사용하는 제 2 단계;
제 1 혼합물 100 중량부에 대해서 충진제 및 증점제를 배합하여 교반하여 제 2 혼합물을 생성하되, 충진제는 탄산칼슘, 탈크, 클레이, 실리카, 산성백토를 포함하는 그룹에서 선택되는 하나 이상이며, 탈크를 이용시 접착제의 성형성과 내가수분해성능을 향상시키기 위하여 첨가되는 것으로, 1액형 접착제 조성물을 구성하는 원재료인 제 1 혼합물 100 중량부에 대하여 충진제 60 내지 65 중량부를 사용하며, 최종 생산되는 피니싱 호일 접착용 친환경 접착제 조성물 용액의 점도를 증가시키기 위한 증점제는 실리카, 흄실리카, 벤토나이트, 클레이, 아마이드, 셀룰로오스로 구성된 그룹에서 선택되는 어느 하나 또는 2종 이상 혼합한 것을 제 1 혼합물 100 중량부에 대하여 증점제 4 내지 7 중량부를 사용하는 제 3 단계;
첨가제로 제 2 혼합물 100 중량부에 대해서 탄소 섬유 24 내지 25 중량부, 난연제 7 내지 10 중량부, 자외선차단제 8 내지 13 중량부, 표면보호제 2 내지 3 중량부를 배합하되, 탄소 섬유는 피니싱 호일과 접착제 조성물 간의 전도성에 따라 용량이 조절되며, 1액형 피니싱 호일 접착용 친환경 접착제 조성물은 탄소 섬유를 첨가 혼합하여 탄소 섬유 강화형(CFR, Garbon Fiber Reinforced Plastic)에 해당하는 레진을 수득하여 사용하며, 난연제는 몰리브덴산 안티몬, 산화몰리브덴, 수산화마그네슘, 수산화알미늄 중 어느 하나 또는 2종 이상 혼합한 것을 사용하며, 자외선차단제는 폴리에틸렌 수지 또는 수성아크릴계 합성수지 100 중량부에 대해서 100 내지 1000㎛의 분체의 평균입도를 갖는 이산화티탄(TiO2) 34 내지 37 중량부와 산화아연(ZnO2) 33 내지 35 중량부를 혼합한 뒤, 혼합물에 감마아미노에틸렌아미노프로필트리메톡시실란의 실란계 화합물 25 내지 27 중량부를 혼합하여 점착성을 부여하고, 혼합 용액에 pH 5 내지 7의 실리콘 오일 2 내지 5 중량부, 계면활성제 2 내지 5 중량부를 혼입하여 15℃ 내지 25℃에서 30분간 교반하여 표면을 개질하여 자외선차단제를 생성하여 사용하는 제 4 단계; 및
상기 제 4 단계의 배합물 100 중량부에 대해서 30 내지 40 중량부의 증류수를 첨가하고, 100 내지 150℃의 온도에서 1 시간 내지 2 시간 사이에서 가열 및 교반하고, 가열 및 교반 완료된 조성물에 대해서 진공탈포하여 접착제 조성물 생성을 완료하는 제 5 단계;
상기 제 5 단계에 따라 생성된 피니싱 호일 접착용 친환경 접착제 조성물을 피니싱 호일이 부착되는 대상에 도포하되 접착력 확보를 위해서 피니싱 호일 및 부착 대상 간의 접착 면에는 에칭(Etching), 코로나 (Corona)처리를 포함한 표면처리를 하여 기계적 맞물림에 따른 앵커링(Anchoring)되도록 하며, 피니싱 호일이 부착되는 대상에 피니싱 호일 접착용 친환경 접착제 조성물을 도포하는 방법은 크게 액형과 고형의 접착제를 사용하는 두 가지 분류로 수행되며 액형의 피니싱 호일 접착용 친환경 접착제 조성물을 도포하는 방법은 스프레이(Spray)나 바코팅(Bar Coating) 방법으로 하거나, 고형의 접착제의 경우에는 피니싱 호일 접착용 친환경 접착제 조성물이 필름 형태로 제조된 것을 이용하여 열압착(thermal lamination) 방법으로 접착하는 제 6 단계; 및
상기 제 6 단계의 피니싱 호일 접합 과정을 거쳐 열간프레스(Hot press) 과정을 수행하되, 피니싱 호일을 접착제가 도포된 부착 대상으로의 접합 과정과 동시에 또는 이후에 열간프레스(Hot press)로 100 ℃이하로 가열, 압착시키며, 1액형 피니싱 호일 접착용 친환경 접착제 조성물은 피니싱 호일의 평량이 30 이상 50g/m2 미만인 경우에는 양을 7 내지 12g/m2로, 피니싱 호일의 평량이 50 이상 70g/m2 미만인 경우에는 양을 10 내지 18g/m2, 피니싱 호일의 평량이 70 이상 100 이하인 경우 양을 17 내지 25m2으로 평량에 따라 접착제 조성물의 양을 가변하여 주는 제 7 단계; 를 포함하는 것을 특징으로 하는 피니싱 호일 접착용 친환경 접착제 조성물의 제조 방법. (PVAc), PVA (Polyvinyl Acetate), PAV (Polyvinyl Alcohol) and PLA (Polyactic Acid) at a weight ratio of 1: 0.8 to 0.9: 0.2 to 0.3. PVA and PLA mixed solution are distributed in more than 60% of the total surface area. The diluent used in the degradation of the capsules is PVA and PLA mixed solution, Polymeric moisture reactive composition that serves as a polymer reactive diluent useful for structural adhesives, which is used to reduce the viscosity of polyvinyl alcohol (PVA), PVAV (Polyvinyl Alcohol), PAV A first step of utilizing a polymer reactive diluent between 5 and 6 wt% based on the total amount of PLA (PolyLactic Acid);
20 to 25 parts by weight of foamed polyethylene particles, 1 to 10 parts by weight of a PHA (polyhydroxyalkanoate) resin, 3 to 20 parts by weight of a water-soluble adhesive (methyl cellulose), 100 parts by weight of a water- 10 to 20 parts by weight of a moisturizer and 2 to 5 parts by weight of a drying agent are mixed to produce a first mixture. The foamed polyethylene particles are prepared by using a polyethylene raw material, Type polyethylene is formed and then formed into a solid form and pulverized into fine particles. The eco-friendly adhesive composition for bonding finishing foil, which is finally prepared, is adhered to an object to be attached, and the weight average molecular weight A melt index of 0.3 to 7 g / 12 min (150 DEG C), a molecular weight distribution (PI) of 5.7 or more, a melt strength of 35 mN or more 12 to 23 parts by weight of a blowing agent are blended with 100 parts by weight of a polyethylene-based raw material. The polyethylene for preparing a foamed polyethylene mixture is used alone or after being foamed after being formed of a polyethylene mixture. The polyethylene mixture is composed of 100 parts by weight of polyethylene 25 to 30 parts by weight of an ethylene-vinyl acetate copolymer (EVA) and 10 to 15 parts by weight of a polyurethane are used for a mixture of PVA, PAV and PLA, and a mixture of foamed polyethylene particles and PHA resin , And water-soluble adhesive (methyl cellulose) were mixed in a mixer while adjusting the temperature of the mixer to 30 to 35 ° C while stirring the mixture for 30 minutes while adding a moisturizing agent (glcerine) ), And the ester is obtained by mixing oleic acid and stearic acid at a ratio of 1: 0.5 to 1 A second step of using;
The filler is at least one selected from the group consisting of calcium carbonate, talc, clay, silica and acidic white clay. The filler is mixed with 100 parts by weight of the first mixture, And 60 to 65 parts by weight of a filler is used for 100 parts by weight of the first mixture, which is a raw material of the one-component adhesive composition, to improve the moldability of the adhesive and the moisture resistance, The thickening agent for increasing the viscosity of the adhesive composition solution is any one selected from the group consisting of silica, fumed silica, bentonite, clay, amide and cellulose, or a mixture of two or more thereof. A third step of using a weight part;
The carbon fiber is mixed with 24 to 25 parts by weight of carbon fiber, 7 to 10 parts by weight of a flame retardant, 8 to 13 parts by weight of an ultraviolet screening agent, and 2 to 3 parts by weight of a surface protective agent per 100 parts by weight of the second mixture, The amount of the environmentally friendly adhesive composition for bonding the one-part finishing foil is adjusted by the conductivity between the compositions. The carbon fiber is added and mixed to obtain a resin corresponding to a carbon fiber reinforced plastic (CFR). The flame retardant Antimony molybdate, molybdenum oxide, magnesium hydroxide and aluminum hydroxide. The ultraviolet screening agent has an average particle size of 100 to 1000 占 퐉 based on 100 parts by weight of the polyethylene resin or the aqueous acrylic resin. titanium dioxide (TiO 2) 34 to 37 parts by weight of zinc oxide (ZnO 2) after mixing 33 to 35 parts by weight, And 25 to 27 parts by weight of a silane compound of gamma aminoethylenaminopropyltrimethoxysilane are mixed to give a tackiness, and 2 to 5 parts by weight of a silicone oil having a pH of 5 to 7 and 2 to 5 parts by weight of a surfactant are added to the mixed solution Mixing and stirring the mixture at 15 ° C to 25 ° C for 30 minutes to modify the surface to produce an ultraviolet screening agent; And
30 to 40 parts by weight of distilled water is added to 100 parts by weight of the blend of the fourth step and heated and stirred at a temperature of 100 to 150 DEG C for 1 to 2 hours and the composition after heating and stirring is vacuum degassed A fifth step of completing the production of the adhesive composition;
The eco-friendly adhesive composition for bonding the finishing foil produced according to the fifth step is applied to an object to which the finishing foil is adhered, and the adhesion surface between the finishing foil and the object to be adhered is etched and corona treated The surface treatment is performed to anchor according to the mechanical engagement and the method of applying the eco-friendly adhesive composition for bonding the finishing foil to the object to which the finishing foil is attached is largely divided into two types using a liquid type and a solid type adhesive, A method of applying an eco-friendly adhesive composition for bonding a finishing foil may be a method of spraying or bar coating or a method of using an eco-friendly adhesive composition for bonding a finishing foil in the form of a film in the case of a solid adhesive A sixth step of bonding by a thermal lamination method; And
The hot pressing process is performed through the finishing foil bonding process of the sixth step and the finishing foil is heated at 100 DEG C or below by a hot press at the same time as or after the bonding process to the object to which the adhesive is applied The amount of the eco-friendly adhesive composition for bonding the one-pack type finishing foil is preferably 7 to 12 g / m 2 when the basis weight of the finishing foil is 30 to 50 g / m 2 , and the basis weight of the finishing foil is 50 to 70 g / m 2 A quantity of 10 to 18 g / m < 2 > when the finishing foil is less than 2, and an amount of the adhesive composition varying from 17 to 25 m < 2 > Wherein the adhesive layer is formed of a thermoplastic resin.