JPS59223370A - Oil agent for treating polyester fiber - Google Patents

Oil agent for treating polyester fiber

Info

Publication number
JPS59223370A
JPS59223370A JP9319283A JP9319283A JPS59223370A JP S59223370 A JPS59223370 A JP S59223370A JP 9319283 A JP9319283 A JP 9319283A JP 9319283 A JP9319283 A JP 9319283A JP S59223370 A JPS59223370 A JP S59223370A
Authority
JP
Japan
Prior art keywords
spinning
oil
oil agent
alkyl
alkyl phosphate
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP9319283A
Other languages
Japanese (ja)
Other versions
JPH0219230B2 (en
Inventor
健次 山本
勝久 田中
吉重 中村
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Matsumoto Yushi Seiyaku Co Ltd
Original Assignee
Matsumoto Yushi Seiyaku Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Matsumoto Yushi Seiyaku Co Ltd filed Critical Matsumoto Yushi Seiyaku Co Ltd
Priority to JP9319283A priority Critical patent/JPS59223370A/en
Publication of JPS59223370A publication Critical patent/JPS59223370A/en
Publication of JPH0219230B2 publication Critical patent/JPH0219230B2/ja
Granted legal-status Critical Current

Abstract

(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。
(57) [Summary] This bulletin contains application data before electronic filing, so abstract data is not recorded.

Description

【発明の詳細な説明】 本発明はポリエステル繊維用紡績油剤に関する。[Detailed description of the invention] The present invention relates to a spinning oil for polyester fibers.

ポリエステル繊維は、単独または櫛、レーヨン、淋、ウ
ールなどの混紡で大量に紡績されているが、近年紡績業
界に2いては紡績コスト低減のために閤能率、省力化が
急務ときれ、このため紡機の高速化と共にこれに適応し
た紡績油剤が強く望まれている。
Polyester fibers are spun in large quantities either alone or in blends with comb, rayon, lintel, wool, etc. In recent years, the spinning industry has seen an urgent need to improve spinning efficiency and save labor in order to reduce spinning costs. As the speed of spinning machines increases, there is a strong desire for a spinning oil that is compatible with this.

紡機の高速化に伴って、静電気の発生によるトラブルや
紡機の繊H,Jff1過部に蓄積するスカムの増加、ロ
ーラー類への捲何増加時のトラブルが発生し易くなるが
、これらトラブルは繊維に(を宥する油剤の種類によっ
て大きく左右される。繊維から脱落して蓄積するスカム
は、コイラーでのチューブ詰シやローラー類への捲付の
原因となシ操菓性を著しく低下させる。また、ゴムロー
ラーの捲付に関しては、スカムの蓄積や油剤の粘着性に
よる捲付の魯ならず、以下に述べるようなローラー表面
の伏態父化も捲付増加の大きな原因になるため、この辿
の捲付も低減されなけれはならない。
As the speed of spinning machines increases, troubles are more likely to occur due to the generation of static electricity, an increase in scum that accumulates on the fibers H and Jff1 of the spinning machine, and troubles when the number of windings on rollers increases. The scum that falls off from the fibers and accumulates can cause tube clogging in the coiler and winding up on rollers, and significantly reduce the confectionery properties. Regarding the winding of rubber rollers, it is important to note that not only the accumulation of scum and the stickiness of the oil agent may cause the winding to increase, but also the fact that the surface of the roller becomes dry as described below. Trace wrapping must also be reduced.

ゴムローラは、一般には捲付減少化のために濃硫酸やそ
の他の薬剤によって表面処理されているが、数カ月紡出
するとその処理効果が失われゴムローラーの表面が処理
前の状態、いわゆる未処理に近い状態になシ、その結果
、ゴムローラーノ捲付が増加し、高湿度の雰囲気ではさ
らに捲付が増加する。このためローラーの交換が必要と
なるが、高速化に伴ってその交換周期は短がくなシ、葦
た錘数が非常に多す粗紡、精紡工程ではローラーの交換
は少なからぬ紡績コスト増につながるため、ローラーの
表面処理効果が低下しても、さらに処理の施されていな
いゴムローラーに2いてもi付が少ない紡績油剤が強く
望丑れる。
Rubber rollers are generally surface treated with concentrated sulfuric acid or other chemicals to reduce wrapping, but after several months of spinning, the treatment effect is lost and the surface of the rubber roller becomes untreated, the so-called untreated state. As a result, wrapping of the rubber roller increases, and wrapping increases even more in a high humidity atmosphere. For this reason, it is necessary to replace the rollers, but as the speed increases, the replacement cycle has to become shorter, and in the roving and spinning processes where the number of reeds and spindles is extremely large, replacing the rollers increases the spinning cost considerably. Therefore, even if the surface treatment effect of the roller decreases, a spinning oil with less i adhesion is strongly desired even if it is attached to an untreated rubber roller.

筒能率、省力化のためには上記のスカムやローラー捲付
を低減させる事は勿論、カード、線条工程で紡出される
スライバーのコイリンク性全向上8?で’y ンy、 
(#1fi) [収容するヌライバーノ嵐全増加させる
事も重要でるる。通常、tj罐もしくは満罐近ぐになる
とコイリングが乱れ、それ以上のスライバーを収容する
事ができなくなるが、コイリングの乱れが発生しなけれ
ばさらにスライバーを収容させる事が可能となり、それ
たけ生産の能率が上るので、目的罐時の繊維−金属間の
接圧の高い状態に2bでもコイリンク在の良い紡績油剤
が益々望まれている。
In order to improve cylinder efficiency and save labor, it is of course necessary to reduce the scum and roller wrapping mentioned above, and to completely improve the coil linking properties of the sliver that is spun in the carding and filament processes8? And'y ny,
(#1fi) [It is also important to increase the number of Nuraibano storms that can be contained. Normally, when the tj can or the can is near full, the coiling becomes disordered and no more sliver can be accommodated, but if the coiling does not become disordered, it becomes possible to accommodate more sliver, which increases production efficiency. Therefore, there is an increasing demand for a spinning oil that has good coil link retention even in 2b, in a state where the contact pressure between the fiber and metal is high in the target can.

ぼた、スライバーの引抜き強力を間めると、それだけ精
紡での撚数を減少させる事が可能となシ、したがって生
産能率が高くなるのでドラフト斑にならない範囲でスラ
イバーの引抜き強力を高める事も能率向上に有効である
By reducing the pulling strength of the sliver, it is possible to reduce the number of twists during spinning, thus increasing the production efficiency, so it is possible to increase the pulling strength of the sliver without causing draft irregularities. is also effective in improving efficiency.

1だ、各紡績工程における雰囲気の温湿)5は紡績性に
大きな影響を与え、通常層温度になるとカード工程での
シリンダー捲付や、線条、粗紡、精紡工程でのゴムロー
ラー捲付が増加し、逆に低湿度になるとn電気の発生や
、繊維−繊維間の抱合性不足あるいは線条工程などでの
ボトム(金属)ローラー捲付ヤチューブ詰り等のトラブ
ルが発生し易くなる。このため紡績調子を良好とするた
めには温湿度を四季を通じて管理する必要かめシ、実際
多くの紡績工場では調tML調湿設踊を置き一定の温湿
度を保つように努めている。しかし、広い紡績工場内の
温湿度を完全に調節する手は離しぐ、また、調温調湿設
備を運転すると多大の費用かがかるため、省エネルギー
コスト低減の怠味から、温湿度の季節的な反動に対して
も紡績調子の艮好な紡績油剤が強く求められている。
1, the temperature and humidity of the atmosphere in each spinning process) 5 has a great effect on spinning properties, and when the layer temperature reaches normal, cylinder winding in the carding process and rubber roller winding in the filament, roving, and spinning processes. conversely, when the humidity is low, problems such as the generation of n-electricity, insufficient conjugation between fibers, and clogging of the bottom (metal) roller winding tube during the filament process are likely to occur. For this reason, in order to maintain good spinning conditions, it is necessary to control temperature and humidity throughout the seasons, and in fact, many spinning factories are equipped with humidity control equipment to maintain a constant temperature and humidity. However, it is difficult to completely control the temperature and humidity inside a large textile factory, and operating temperature and humidity control equipment costs a lot of money. There is a strong demand for a spinning lubricant that provides good spinning performance even against recoil.

従来、ポリエステ/l/滅a用の油剤としてはアルキル
燐酸エステルNk主成分とするものが広く用いられてき
たが、実用上、最もよく使用されているものはラウリル
アルコールの燐酸エステルであシ、アルキル基の炭素数
は多くてせいぜい16であって、炭素数18以上のアル
キル燐酸エステルは実用的には殆んど無視されていた。
Conventionally, oils containing alkyl phosphate esters (Nk) as the main component have been widely used as oils for polyester/l/aerosols, but in practice, the most commonly used oils are lauryl alcohol phosphate esters, The number of carbon atoms in the alkyl group is at most 16, and alkyl phosphates having 18 or more carbon atoms have been practically ignored.

その埋出は炭素数の多い、例えば18以上のアルキル燐
酸エステルは水浴性が低く使用が不便でろシ、かつその
様に炭素数の多いアルキル燐酸エステルを用いても炭素
数16以下のアルキル燐酸エステルに比べて格別優れた
効果が達成されるとは期待されていなかったためと考え
られる。
For example, alkyl phosphate esters with a large number of carbon atoms, such as alkyl phosphate esters with a carbon number of 18 or more, have poor water bathability and are inconvenient to use. This is thought to be because it was not expected to achieve particularly superior effects compared to the previous one.

上記のごとき従来のアルキル燐酸エステル橿を主成分と
するポリエステル繊維用処理剤は迩切な温湿度条件下で
はローラー捲付が少ないと云う長所を有するが、面温度
ではローラー捲付が多く、互た低臨時では制電性や繊維
の集束性が悪いなど紡績性の1M湿度依存性が大きく、
しかもオープンエンドMvJに適用したときはなおスカ
ム防止が十分てない等の欠点かめる。さらに前述の表面
処理効果のなくなったゴムローラーに対しては捲付が多
く、また直湿下においては吸湿によって旧イ1jの粘着
性が大きくなるため、スカムの蓄績やローラー捲付が多
くなる。
Conventional polyester fiber treatment agents containing alkyl phosphate esters as the main component have the advantage of less roller wrapping under moderate temperature and humidity conditions; At low temporary properties, the spinnability is highly dependent on 1M humidity, such as poor antistatic properties and poor fiber cohesiveness.
Moreover, when applied to open-end MvJ, there are still drawbacks such as insufficient scum prevention. Furthermore, the rubber rollers that have lost their surface treatment effect tend to get wrapped around more often, and in direct humidity, the adhesiveness of the old I1J increases due to moisture absorption, resulting in more scum accumulation and roller wrapping. .

特公昭57−37707号公報はアルキル燐酸エステル
と特定の酸化エチレン付加モル数のポリオキシエチレン
アルキルエーテル(エヌプール)および脂肪酸エステル
とを特定の割合で配合した紡績油剤を開示している。こ
の紡績油剤はコーミングローラ−への捲付の少なめアル
キル燐酸塩とスカム発生の少ない特定の非イオン界面活
性剤釈よび両者に対し相溶性である脂肪酸エヌテル全用
いて、スカムの発生とローラーへの捲付を防止すること
を目的とする。しかしながら、この紡績油剤も本質的に
は従来の炭素数12〜16のアルキル燐酸エステル系の
ものであって、スカムの発生とローラーへの捲付をアル
キル燐酸エステルと非イオン界面活性剤と全特定の配合
比で配合することにより解決しているにすき゛ない。確
かに上記公報にはステアリルホスフェートの記載はめる
が、その使用重は60M量%を越えて用いることはでさ
ない。従って、温湿度の季節的変動に影響されず、カッ
米処理ゴムローラーへの捲付防止効果は得られない。
Japanese Patent Publication No. 57-37707 discloses a spinning oil containing an alkyl phosphate ester, a polyoxyethylene alkyl ether (N-pur) having a specific number of added moles of ethylene oxide, and a fatty acid ester in a specific ratio. This spinning oil uses an alkyl phosphate that reduces the amount of scum that gets wrapped around the combing roller, a specific nonionic surfactant that reduces scum generation, and a fatty acid ether that is compatible with both of them. The purpose is to prevent wrapping. However, this spinning oil is essentially a conventional alkyl phosphate ester with a carbon number of 12 to 16, and the generation of scum and its wrapping around the rollers are completely identified as alkyl phosphate esters and nonionic surfactants. It would be better if the problem could be solved by blending at the blending ratio of . It is true that stearyl phosphate is mentioned in the above-mentioned publication, but its usage weight cannot exceed 60 M%. Therefore, it is not affected by seasonal fluctuations in temperature and humidity, and the effect of preventing wrapping around the rice processing rubber roller cannot be obtained.

本発明は尚湿時に2いても紡績工程でのローラー捲付が
少なく、スカムの発生が少なく、かつ刀−ド、練条工程
で紡出されるスライバーのコイリング性向上によってケ
ンス収容量の増加全可能にし、さらにスライバーの引抜
き強力を高めることによって、稍tjに寂ける撚数全減
少せしめて生産効率を旨め、同時に温湿度灰化に関係な
く艮好な紡績性全付与する紡績油剤を提供する。
The present invention has less roller wrapping during the spinning process even when it is humid, less scum generation, and improved coiling properties of the sliver spun in the sword and drawing processes, making it possible to increase the capacity of the can. To provide a spinning oil agent which improves production efficiency by completely reducing the number of twists that are slightly dull by increasing the pulling strength of the sliver, and at the same time imparts excellent spinning properties regardless of temperature and humidity. .

即ち、本発明は、炭素数が18〜20である協和の高級
アルコールの1榎または2棟以上を50M重%以上含有
し、かつ全アルキル基の平均炭素数が17〜21の範囲
にめる直鎮および/葦たは111鎖を有する高級アルコ
ールの燐酸エステル化物を、無機アルカリ水酸化物で中
和して得られるアルキル燐酸エステルの金ノ萬塩を60
重重%より多く含有するポリエステル繊維処理用油剤に
関する。
That is, the present invention contains one or more of Kyowa's higher alcohols having 18 to 20 carbon atoms in an amount of 50M weight or more, and the average carbon number of all the alkyl groups is in the range of 17 to 21. 60% gold salt of alkyl phosphate obtained by neutralizing a phosphoric acid ester of a higher alcohol having 111 chains and/or 111 chains with an inorganic alkali hydroxide.
This invention relates to an oil agent for treating polyester fibers containing more than % by weight.

本発明において使用するアルキル燐酸エステルの金属塩
は、炭素数18〜20の飽和高級アルコールの1佳又は
2種以上を50恵量%以上含有して、全アルキル基の平
均炭素数が17より大さく21より小さい範囲にめる直
頑互たは/2よび側順を有する高級アルコールの燐酸エ
ステル化によって得られる燐酸化度(アルコール1モル
に結合する燐原子のダラム原子数)0.6〜1.2の酸
性アルキル燐酸エステルを無機アルカリ水酸化物で中和
して得られる。
The metal salt of alkyl phosphate used in the present invention contains 50% or more of one or more saturated higher alcohols having 18 to 20 carbon atoms, and the average carbon number of all the alkyl groups is greater than 17. Phosphorylation degree (Durham number of phosphorus atoms bonded to 1 mole of alcohol) obtained by phosphoric acid esterification of higher alcohols having direct rigidity or /2 and side order in a range smaller than 21 0.6 ~ It is obtained by neutralizing the acidic alkyl phosphate ester of 1.2 with an inorganic alkali hydroxide.

本発明のアルキル燐酸エステルに使用される原料アルコ
ールとしては、例えばヌテアリルアルコール、インヌテ
アリルアルコール、ノナデシルア       □)ル
コール、エイコシルアルコール等かめルカ、コれら単独
でもブレンドしても艮い。わるいなまた、炭素数18〜
20と炭素数17以下のアルコール、例えは、〆′セチ
ルアルコールなトラ含むアルコールであっても、前記の
要件を瀾たすような、即ち炭素数18以上のアルキル基
が50%以上となるようなアルコールでめれば使用する
事がでさ、ブレンドであっても、天然から誘導されるア
ルコール、例えば牛脂還元アルコールであっても艮い。
The raw material alcohol used for the alkyl phosphate ester of the present invention includes, for example, nutaryl alcohol, inutearyl alcohol, nonadecyl alcohol, eicosyl alcohol, etc., and these may be used alone or as a blend. Also, carbon number is 18~
20 and an alcohol having 17 or less carbon atoms, for example, even if it is an alcohol containing a tera such as cetyl alcohol, the alcohol must meet the above requirements, that is, the alkyl group having 18 or more carbon atoms should account for 50% or more. It can be used as long as it is mixed with alcohol, whether it is a blend or a naturally derived alcohol, such as reduced beef tallow alcohol.

1だ、炭素数18〜20と炭素数21以上のアルコール
、例、t ハトコシルアルーコールなどを含むアルコー
ルであっても、前記の要件ヲ瀾だしていれば使用するこ
とができる。炭素数17以下のアルコールを含有する場
合は、炭素数18〜20のアルコールは飽和である事が
望ましい。1だ、不飽和アルコールトシて、例えばオレ
イルアルコール、リルイルアルコール、リルニルアルコ
ール等に50%以下、好1しくに30%以下の範囲でブ
レンドする事ができるが、@植物前から誘導されるアル
コールを部分還元したものでも前記の要件を1tj足し
ていれば使用する事ができる。平均炭素数が21より大
きくなると水に対する溶解性が悪くなり、繊維への均一
な給量が媒しくなる。fだ、飽和アルキルが50%よシ
少ない場合は高m1時の油剤の粘着性が大さくなシ、ス
カム増加やローラー捲付の原因となる。
1. Even alcohols containing 18 to 20 carbon atoms and 21 or more carbon atoms, such as t-hatocyl alcohol, can be used as long as they meet the above requirements. When containing an alcohol having 17 or less carbon atoms, it is desirable that the alcohol having 18 to 20 carbon atoms is saturated. 1. Unsaturated alcohols, such as oleyl alcohol, lylyl alcohol, lylunyl alcohol, etc., can be blended in an amount of 50% or less, preferably 30% or less, but are derived from plants. Partially reduced alcohol can also be used as long as it meets the above requirements by 1tj. When the average carbon number is greater than 21, the solubility in water becomes poor, making it difficult to uniformly feed the fibers. f. If the saturated alkyl content is less than 50%, the viscosity of the oil at high m1 will be low, causing an increase in scum and roller wrapping.

また、アルキル燐酸エステル金属塩のアルカリ金属はリ
チウム、ナトリウム、カリウムなどであるが、制電性の
点から特にカリウムが良く、また中和の程度は制電性の
点から酸性アルキル燐酸エステルの全酸基の60〜10
0%当重、好1しくは70〜100%当量であシ、60
%当量よシ低い場合は制電性が不良となる。
In addition, the alkali metal of the alkyl phosphate metal salt is lithium, sodium, potassium, etc., but potassium is particularly good from the viewpoint of antistatic properties, and the degree of neutralization is determined from the viewpoint of antistatic properties. 60-10 acid groups
0% equivalent weight, preferably 70-100% equivalent weight, 60
If it is lower than % equivalent, the antistatic properties will be poor.

上記の如く合成されたフルキルS酸エヌテル金属橿は劉
温高湿時においても性状が梗く、吸湿による粘着性も非
常に小さいのでスカムの蓄積が著しく低減される。また
、表面処理式れたゴムローラーのみならず未処理のゴム
ローラーに対する両温時の捲付も極めて少なく、温湿度
に鈍感であシ、更にはスライバーの引抜き強力が局いと
いう特畝を有して′J?シ、紡績油剤の主要成分として
非常に優れている。ゴムローラー特に未処理のゴムロー
ラーに対する捲付は油剤の粘着性の大小と必ずしも相関
するものではなく、本発明のアルキル燐酸エステル金属
塩の捲付が少ない理由は、単に粘着性が小さいという事
だけでなく油剤とゴム間の相互作用も大ぎ〈関係してい
る。
The furkyl S-acid Nether metal rod synthesized as described above maintains its properties even under high temperature and high humidity conditions, and has very low stickiness due to moisture absorption, so that the accumulation of scum is significantly reduced. In addition, it has a special ridge that has extremely little winding at both temperatures, not only on surface-treated rubber rollers but also on untreated rubber rollers, and is insensitive to temperature and humidity. 'J? It is excellent as a main component of textile oil. The sticking of rubber rollers, especially untreated rubber rollers, does not necessarily correlate with the level of tackiness of the oil, and the reason why the alkyl phosphate metal salt of the present invention hardly sticks is simply that the tackiness is low. In addition, the interaction between the oil and rubber is also closely related.

本発明にPいて上記アルキル燐酸エステル塩は油剤固形
分全量の60重量%よシ多く、好lしくは65〜90嵐
嵐%使用する。もちろん100恵量%使用してもよい。
In the present invention, the alkyl phosphate ester salt is used in an amount of more than 60% by weight, preferably 65 to 90% by weight, based on the total solid content of the oil agent. Of course, you can use 100%.

60重蛍%以下で使用する場合は、他の配合剤の欠点が
表われるため打丁しくない。
If it is used at a concentration of 60% or less, it will not be suitable for cutting because the drawbacks of other ingredients will appear.

本発明ポリエステル繊維処理用油剤には他の成分、例え
ば集束剤、平滑剤、制′成剤等を配合してもよい。但し
その量は全固形分の40重量%未満好ましくは35重量
%以下にとどめるのが好1し寵 巣果剤としてはポリオキシアルキレンアルキルエーテル
、ポリオキシアルキレンアルケニルエーテル、ポリオキ
シアルキレンアルキルアリールエーテル、等でメジ、ポ
リオキシアルキレンとじてはポリオキシエチレンおよび
/1だにポリオキシプロピレンを示す。ポリオキシアル
キレン付加モル数は特に限定的ではないが1〜50.特
に3〜25でめる。ポリオキシエチレンとポリオキシア
ルキレン両者が付加した場合はランタム土台またはブロ
ックM合いずれであってもよい。
The oil agent for treating polyester fibers of the present invention may contain other components such as a sizing agent, a smoothing agent, and a control agent. However, the amount thereof is preferably kept at less than 40% by weight of the total solids, preferably 35% by weight or less. Examples of the additives include polyoxyalkylene alkyl ether, polyoxyalkylene alkenyl ether, polyoxyalkylene alkylaryl ether, Polyoxyalkylene refers to polyoxyethylene and /1 refers to polyoxypropylene. The number of moles of polyoxyalkylene added is not particularly limited, but is 1 to 50. Especially between 3 and 25. When both polyoxyethylene and polyoxyalkylene are added, either a lantum base or a block M combination may be used.

アルキル基またはアルケニル基の炭素数は8〜18、ア
ルキルアリール基は合計の炭素数14〜28が適当であ
る。
It is appropriate that the alkyl group or alkenyl group has 8 to 18 carbon atoms, and the alkylaryl group has a total of 14 to 28 carbon atoms.

集束剤としての別の列は側鎖および/Iたは不飽和基を
有してもよい伏索逐8〜18のカルボン酸と多1曲アル
コール ル、ポリアルキレングリコール(好葦しくに厘合度50
以下)、グリセリン、ンルビト−ル、ンルビタン、ペン
タエリスリトール、ポリグリ士リン等、アルキレングリ
コールとしてはエチレンクリコール、プロピレングリコ
ール、ポリアルキレングリコールとしてはポリエチレン
クリコール、ポリプロピレングリコール葦たはそれらの
ブロック葦たにランダム重合体等のモノ、またはジエス
テルである。
Another class of sizing agents are carboxylic acids and polyalcohols, polyalkylene glycols, which may have side chains and/or unsaturated groups. 50
(below), glycerin, nrubitol, nrubitan, pentaerythritol, polyglycerin, etc. Alkylene glycols include ethylene glycol, propylene glycol, polyalkylene glycols include polyethylene glycol, polypropylene glycol reeds or block reeds thereof. It is a mono or diester such as a random polymer.

集束剤の典型的な例はポリオキシエチレンラウリルエー
テル、ポリオキシエチレンヌテアリルエーテル、ポリオ
キシエチレンオレイルエーテル、ポリオキシエチレンポ
リオキシプロビレン(ブロック)インオクチルエーテル
、ポリオキシエチレンノニルフェニルエーテル、ホリオ
キシエチレンドデシルフェニルエーテル、ポリエチレン
グリコールモノラウレート、ポリエチレングリコールジ
オレート、ポリオキシエチレン ポリオキシプロピレン
 ステアレート、ラウリン酸ジグリセライド、ヌテアリ
ン酸モノグリセライド、オレイン酸モノグリセライド、
ンルビタンシラウレート、ンルビタンモノステアレート
等が6る。
Typical examples of sizing agents are polyoxyethylene lauryl ether, polyoxyethylene nutearyl ether, polyoxyethylene oleyl ether, polyoxyethylene polyoxypropylene (block)inoctyl ether, polyoxyethylene nonylphenyl ether, holoxy Ethylene dodecyl phenyl ether, polyethylene glycol monolaurate, polyethylene glycol diolate, polyoxyethylene polyoxypropylene stearate, lauric acid diglyceride, nutearic acid monoglyceride, oleic acid monoglyceride,
Examples include nrubitan silaurate and nrubitan monostearate.

平滑剤としてはifll順および/″′!.たは不飽和
基を有していてもよい炭素数8〜18のカルボン酸とi
fll 頑!−よび/または不朗和基を有していてもよ
い7yコールとのエステル(アルキルアルキレート)i
illl頑および/葦たは不飽和基を有していてもよい
炭素数8〜18の高級アルコールと多価カルボン酸、例
えばフタル酸、トリメリット酸、マレイン酸、アジピン
w!等のモノ、シ、トリエステル(多価酸エステル)が
例示される。
As a smoothing agent, a carboxylic acid having 8 to 18 carbon atoms which may have an ifll order and /'''!. or an unsaturated group and i
flll stubborn! - Esters (alkyl alkylates) with 7y alcohols which may have - and/or undesirable groups
Higher alcohols with 8 to 18 carbon atoms which may have strong and/or unsaturated groups and polycarboxylic acids such as phthalic acid, trimellitic acid, maleic acid, adipine w! Examples include mono-, di-, and triester (polyhydric acid ester).

アルキルアルキレートとしては、メチルラウレート、ブ
チルラウレート、インオクチルパルミテート、ラウリル
オレート、インステアリルオレート、オレイルオレート
等がめシ、多塩基酸のエステルとしては、ジオクチルフ
タレート、トリオクチルトリメリテート、モノオクチル
マレート、ジオクチルマレート、シインスークチルアシ
ベート等かめる。
Examples of alkyl alkylates include methyl laurate, butyl laurate, inoctyl palmitate, lauryl oleate, instearyl oleate, and oleyl oleate; examples of esters of polybasic acids include dioctyl phthalate, trioctyl trimellitate, and Contains octyl maleate, dioctyl maleate, cyine suctyl acybate, etc.

i[ilJ 型剤トしてはポリオキシアルキレンアルキ
ル(互りはアルケニル)アミン、!4級アンモニウム塩
が例示される。ポリオキシアルキレンアルキ/I/(i
たはアルケニル)アミンとしてはエチレンオキシドおよ
び/葦たはフ″ロピレンオキシド付7mーr=iv数2
〜50、特に5〜35の炭素数8〜18の911 順’
に有していてもよいアルキルまたはアルケニルアミン、
例えばポリオキシエチレンラウリルアミン、ポリオキシ
エチレンステアリルアミン、ポリオキシエチレンオレイ
ルアミン、ポリオキシエチレンポリオキシプロピレン(
ブロック)ミリヌチルアミン等が例示される。
i [ilJ Type agent is polyoxyalkylene alkyl (alkenyl) amine,! Quaternary ammonium salts are exemplified. Polyoxyalkylenealkyl/I/(i
or alkenyl) amine with ethylene oxide and/or fluoropylene oxide 7mr=iv number 2
~50, especially 5 to 35 carbon atoms 8 to 18 911 order'
an alkyl or alkenylamine which may have
For example, polyoxyethylene laurylamine, polyoxyethylene stearylamine, polyoxyethylene oleylamine, polyoxyethylene polyoxypropylene (
Block) Millinutylamine etc. are exemplified.

第4級アンモニウム塩としては一般式:〔式中、klは
倶j頂2よび/葦たは不飽和基を有していてもよい炭素
1;!17〜17のアルキル基、Zは−CH・ −CO
NH(CH2) 1〜3・R2・R3− およびR4は同一または異ることもめるメチル、エチル
2よびヒドロキシエチル基υよびxHアニオン残基を表
わす〕で表わされる化合物が好ましい。
The quaternary ammonium salt has the general formula: [In the formula, kl is 2 atom(s) and/or 1 carbon which may have an unsaturated group;! 17 to 17 alkyl group, Z is -CH/-CO
A compound represented by NH(CH2) 1-3.R2.R3- and R4, which may be the same or different, represents methyl, ethyl 2, a hydroxyethyl group υ, or an xH anion residue is preferred.

第4級アンモニウム塩としてはラウリルジメチルエチル
アンモニウムエトサルフェート、ステアリルトリメチル
アンモニウムメトサルフェート、N、N−ジメチル−N
−2−ヒドロキシエチル−N−オレオイルアミドプロピ
ルアンモニウムナイトレート等がある。
Quaternary ammonium salts include lauryldimethylethylammonium ethosulfate, stearyltrimethylammonium methosulfate, N,N-dimethyl-N
-2-hydroxyethyl-N-oleoylamidopropylammonium nitrate and the like.

集束剤、平滑剤および制電剤の配合比はそれぞれ繊維処
理用油剤全固形分の10〜35重量%、0〜20重量%
2よび0〜20恵試%が好ましい。
The blending ratio of the sizing agent, smoothing agent, and antistatic agent is 10 to 35% by weight and 0 to 20% by weight of the total solids of the fiber treatment oil, respectively.
2 and 0-20 % are preferred.

本究明の油剤は水で希釈したエマルシ゛ヨンとして用い
る事が望ましく、このエマルゾョンを紡糸、延伸及びそ
の他の給油工程で、浸漬、スプレー葦たばその他の方式
によってトウ葦たはヌテーブルファイバー状のものにイ
」盾ざゼて処理する。互だ、〕ぜi染の場合は染色工程
でも処理する串ができる。
It is preferable to use the oil agent of the present invention as an emulsion diluted with water, and this emulsion is transformed into tow reed or nutable fiber by dipping, spraying, or other methods during spinning, drawing, and other oiling processes. I'll handle it with a shield. ] In the case of Zei dyeing, skewers are also produced during the dyeing process.

本発明油剤の繊維に対する付1¥を斌は0.05〜1重
量%、好1しくに0.08〜0.3厘量%でめる。
The amount of the lubricant of the present invention applied to the fiber is 0.05 to 1% by weight, preferably 0.08 to 0.3% by weight.

尚、本発明油剤には他の紡績油剤あるいは防腐剤、防錆
剤、染料等の助剤を本発明の効果を失わない限り添加す
る事かでさる。
In addition, other spinning oils or auxiliary agents such as preservatives, rust preventives, dyes, etc. may be added to the oil of the present invention as long as the effects of the present invention are not lost.

以下、本発明全突施例を挙げて説明するが、本発明はこ
れら実施例によって何等1flJ眠を受けるものではな
い。
Hereinafter, the present invention will be explained with reference to all embodiments, but the present invention is not limited in any way by these embodiments.

実施例1 表−1に示す本発明のアルキル燐酸エステル橿と比軟油
剤を80℃で2時間、さらに60℃で6時間真空乾燥し
た絶乾試料を、20℃×65%RH2よび30℃X80
%RHの温湿度下に置いて4日間調温調湿した後、性状
を判定した。その結果を表−1vc示す。
Example 1 A bone dry sample obtained by vacuum drying the alkyl phosphate ester and specific oil softening agent of the present invention shown in Table 1 at 80°C for 2 hours and further at 60°C for 6 hours was dried at 20°C x 65% RH2 and at 30°C x 80°C.
After placing it under a temperature and humidity of %RH and controlling the temperature and humidity for 4 days, the properties were determined. The results are shown in Table 1vc.

表−1 表−1から、本発明のアルキル燐酸エステル塩は高温品
温下においてもI!+:、伏の便化かほとんどなく、粘
看性のない映い固状でめるので温湿度に対して極めて鈍
16でめる叩が分かる。比軟のラウリル騎酸エヌテルに
橿は高温品温になると#’+!i 3W性のめるペース
ト状に友化し、温湿度の影響金受は易い。1だ、ノニオ
ン系のl田斤14 Yは温湿度に鈍1悠でるるが、後記
の表−3に示すようにカード工程でシリンダー捲付が発
生する。
Table 1 From Table 1, it can be seen that the alkyl phosphate ester salt of the present invention has I! +: There is almost no melting, and it is solid with no viscosity, so it can be seen that it is very sensitive to temperature and humidity. When it comes to the high temperature of the soft lauryl dicarboxylic acid N'TEL, it's #'+! i 3W properties make it into a paste-like form, and it is easily absorbed by temperature and humidity. 1, nonionic lada 14 Y is sensitive to temperature and humidity, but as shown in Table 3 below, cylinder wrapping occurs during the carding process.

実施例2 ポリエステルヌテープ(1,3dX38m)に対し、表
−2に示す本発明油剤A2よびE〜■並ひに比軟の油I
IJ X −Z ’(5それぞれ浸漬法で油剤付着量が
0.13%(重重)になるように付層させて80℃;で
乾燥し、20℃×45%RH120℃×65%RHi−
よび30℃×80%KHで24時間調温調湿した後、ミ
ニチュアタイプの紡機によって下a己項目を評1曲した
。その子百呆を表−3に示す。
Example 2 Polyester tape (1.3 d x 38 m) was treated with oils A2 and E of the present invention shown in Table 2 as well as relatively soft oil I.
IJ
After controlling the temperature and humidity at 30° C. and 80% KH for 24 hours, the following items were evaluated using a miniature spinning machine. Table 3 shows the child's confusion.

(1)カード工程での制電性: ウェブ上の光生静醒気(帯′紙圧)全を日式果電器で測
定した。
(1) Antistatic properties in the carding process: The total photogenic static air (band's paper pressure) on the web was measured using a Japanese-style photometer.

(2ンカード工程でのシリンタ゛−捲付:ステーブル リンダー捲付1陽を測定してシリンダー幅に対する自分
率で示した。
(Cylinder winding in the 2-linked process: Stable cylinder winding 1 yen was measured and expressed as a ratio to the cylinder width.

(3)線条ローラー捲付: カード上りのウェブ全ドラムに捲取ったものを3個作り
(40y−X3)、これを線条優にかけてつなぎ1本の
スライバーとした後、紡出グレン約180/6ヤードで
4回株返し線条し、処理(硫酸)ゴムローラーに対する
捲付回数を測定した。
(3) Winding with a filament roller: Make three pieces (40y-X3) by winding the entire web of the carded web onto the drum, and after splicing this with filament yarn and making it into one sliver, the spinning grain is approximately 180. The stock was returned and striated 4 times at /6 yards, and the number of times it was wrapped around a treated (sulfuric acid) rubber roller was measured.

(滲スライバーの引抜き強カニ 線条上夛のスライバーの引抜き強力全ドラフト・−トチ
スターで測定した後、この実lllllI値を測定L7
+りL L/たスライバ−の重量で割り、単位重量当り
の引抜き強力として示した。
(Strong pulling of the sliver on the crab filament) Strong pulling of the sliver on the crab filament After measuring with a full draft, the actual llllllI value was measured L7
It is expressed as the drawing strength per unit weight, which is divided by the weight of the sliver.

(5)精紡ローラー捲付: 線条上りのスライバーをスーパーハイトラフトタイプの
稍紡楓にかけ、糸を切断した状態で未処理状態のゴムロ
ーラーに対する捲付を測定した。捲付は30分当シの捲
付ljlliJ数で示した。
(5) Winding on a spinning roller: A filamented sliver was passed through a super-high-traft type fine spinning maple, and the winding on an untreated rubber roller was measured with the yarn cut. The winding is indicated by the number of windings per 30 minutes.

表−2(つづき) 表−3 表−3から明らかなように、本発明油剤はゴム・ローラ
ーの処理、未処理に関係なく捲付か非常に少なく、スラ
イバーの引抜き強力も比較のラウリル燐酸エヌテル橿を
主成分とした組成に比べて大きく、1だ制X件やカード
通過性も良好でるる。
Table 2 (Continued) Table 3 As is clear from Table 3, the oil of the present invention has very little curling, regardless of whether the rubber roller is treated or untreated, and its sliver pulling strength is also higher than that of the lauryl phosphate entel roller. It is larger than the composition mainly composed of , and has good 1-dose system and card passability.

実施例3 表−2の本発明油剤EとGおよび比奴の油剤Zを実施例
2と同様にして給油、調製したステープル3即をカード
、線条本機にかけ、コイリング性とスカムを評価した。
Example 3 The present invention lubricants E and G in Table 2 and Hiku's lubricant Z were applied in the same manner as in Example 2, and the prepared staple 3 was applied to a card and filament machine to evaluate coiling property and scum. .

その結果を表−4に示す。The results are shown in Table-4.

本発明油剤はコイリング性(コイル形状)、ヌカム共優
れている事が明らかである。
It is clear that the oil of the present invention has excellent coiling properties (coil shape) and consistency.

※スカムは線条上シのヌライバーtガイドを繰返し通し
てガイドに蓄積するヌカムidk肉眼で観察した。
* Scum was observed with the naked eye by repeatedly passing through the Nuribar T guide on the striae and accumulating on the guide.

◎ 非常に良い  O良い  × 悪い手続補正書(自
発) 特許庁 長官 殿 1事件の表示 昭和58年特許願第  93192    号2発明の
名称 ポリエステル繊維処理用油剤 3補正をする者 事件との関係 特許出願人 4代理人 住所 大阪府大阪市東区本町2−10 本町ビル内6、
補正の対象 明細書の「発明の詳細な説明」の欄7、補
正の内容 (1)明細書第18頁末第10行、[ポリエステルステ
ー1」とある全「ポリエステルステープル」に訂正する
◎ Very good O Good × Bad Procedural amendment (voluntary) Director General of the Patent Office 1 Display of the case 1982 Patent Application No. 93192 2 Name of the invention Oil agent for treating polyester fibers 3 Relationship with the amended case Patent application Person 4 Agent Address: 6 Honmachi Building, 2-10 Honmachi, Higashi-ku, Osaka City, Osaka Prefecture.
Target of amendment Column 7 of the "Detailed Description of the Invention" of the specification, contents of the amendment (1) In the 10th line at the end of page 18 of the specification, the entire text "Polyester Staple 1" is corrected to "Polyester Staple."

(2)同第22頁表−3、評価項目中、[シリンダー捲
付(回)」とある全1シリンダー捲付(%)」に訂正す
る。
(2) In Table 3 on page 22, in the evaluation items, the phrase ``Cylinder wrapping (times)'' has been corrected to ``Total 1 cylinder wrapping (%)''.

以上that's all

Claims (1)

【特許請求の範囲】 1、炭素数が18〜20である飽和の同級アルコールの
1種または2棟以上を50電量%以上含有し、かつ全ア
ルキル基の平均炭素数が17〜21の範囲にめる石鯛お
よび/lたは狽1j頑を有する高級アルコールの燐酸エ
ステル化物を、無機アルカリ水酸化物で中和して得られ
るアルキル燐酸エステルの金属塩を60重量%よシ多ぐ
含有するポリエステル繊維処理用油剤。 2、 アルキル燐酸エステルの金属塩を65重量%以上
含有する第1項記載の油剤。 3、 アルキル燐酸エステルが全酸基の60〜100%
中和されている第↓項記戦の油剤。 4、金属塩がカリウム塩である第1項記載の油剤。
[Scope of Claims] 1. Contains 50% or more of one or more saturated homogeneous alcohols having 18 to 20 carbon atoms, and the average carbon number of all alkyl groups is in the range of 17 to 21. A polyester containing more than 60% by weight of a metal salt of an alkyl phosphate obtained by neutralizing a phosphoric acid ester of a higher alcohol with an inorganic alkali hydroxide. Oil agent for textile processing. 2. The oil agent according to item 1, which contains 65% by weight or more of a metal salt of an alkyl phosphate ester. 3. Alkyl phosphate ester accounts for 60-100% of the total acid groups
The oil of war described in section ↓ has been neutralized. 4. The oil agent according to item 1, wherein the metal salt is a potassium salt.
JP9319283A 1983-05-26 1983-05-26 Oil agent for treating polyester fiber Granted JPS59223370A (en)