JPH0859981A - Moisture-permeable urethane-based elastomer film - Google Patents

Moisture-permeable urethane-based elastomer film

Info

Publication number
JPH0859981A
JPH0859981A JP21521094A JP21521094A JPH0859981A JP H0859981 A JPH0859981 A JP H0859981A JP 21521094 A JP21521094 A JP 21521094A JP 21521094 A JP21521094 A JP 21521094A JP H0859981 A JPH0859981 A JP H0859981A
Authority
JP
Japan
Prior art keywords
film
weight
moisture
polyurethane resin
polyether
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP21521094A
Other languages
Japanese (ja)
Inventor
Hidenori Ishizuka
英紀 石塚
Hideaki Toda
英明 戸田
Kenji Miyasaka
健司 宮坂
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Tonen Chemical Corp
Original Assignee
Tonen Sekiyu Kagaku KK
Tonen Chemical Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Tonen Sekiyu Kagaku KK, Tonen Chemical Corp filed Critical Tonen Sekiyu Kagaku KK
Priority to JP21521094A priority Critical patent/JPH0859981A/en
Publication of JPH0859981A publication Critical patent/JPH0859981A/en
Pending legal-status Critical Current

Abstract

PURPOSE: To prepare a urethane-based elastomer film, having good moisture permeability and waterproofness, improved in moldability through increasing its melt-tension and its blocking resistance, etc., in particular, surpassing the level of a moisture permeability of >=2000g/m<2> .24hrs. and that of a water resistance of >=1000mmH2 O considered as the respective targets in the diaper field, by using a polyether-based thermoplastic polyurethane excellent in mechanical strength and stretchability. CONSTITUTION: This elastomer film is prepared by film-formation of a thermoplastic elastomer composition obtained by blending 5-40 pts.wt. of a filler with 100 pts.wt. of a polyurethane-based resin composition comprising 75-95wt.% of a thermoplastic polyurethane resin with the soft segments consisting of a polyether and 5-25wt.% of an ethylene-propylene-diene copolymer rubber.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は、ウレタン系エラストマ
ーフイルムに関し、特に、オムツのギャザー、バックシ
ート等の衛生材料分野、コート等の衣料分野等におい
て、就中、透湿性、防水性の具備を必要とする分野にお
いて有効に使用できるウレタン系エラストマーフイルム
に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a urethane elastomer film, and more particularly, it has moisture permeability and waterproofness in the fields of sanitary materials such as gathers and back sheets of diapers, and clothing such as coats. The present invention relates to a urethane-based elastomer film which can be effectively used in a required field.

【0002】[0002]

【従来の技術】従来の透湿性ウレタンフイルムの製造方
法としては、ポリエーテル系熱可塑性ポリウレタンを用
い、特開昭62−290714号公報に記載されている
ような連続コーティング装置を用いて、ポリウレタン重
合体の溶媒溶液を離型紙に塗布し、次いで、乾燥炉中を
通過させて溶媒を乾燥させた後、形成されたフイルムを
離型紙から剥離せずにあるいは剥離して巻取ロールに巻
き取る方法がある。しかし、当該ポリウレタン重合体の
溶媒溶液を離型紙に塗布し、溶媒を乾燥させてウレタン
フイルムを得る方法は、溶媒の回収、乾燥工程等が必要
で、コスト高につながり、生産性にも問題がある。
2. Description of the Related Art As a conventional method for producing a moisture-permeable urethane film, a polyether-based thermoplastic polyurethane is used, and a polyurethane coating is carried out by using a continuous coating apparatus as described in JP-A-62-290714. A method in which the combined solvent solution is applied to release paper, and then the solvent is dried by passing through a drying oven, and then the formed film is not peeled from the release paper or is peeled off and wound onto a take-up roll. There is. However, a method of applying a solvent solution of the polyurethane polymer to release paper and drying the solvent to obtain a urethane film requires recovery of the solvent, a drying step, and the like, which leads to high costs and problems in productivity. is there.

【0003】また、熱可塑性ポリウレタンエラストマー
は、粘着性が高く、ブロッキングし易く、溶融張力が低
いため、そのもの単独では、キャスト法やインフレーシ
ョン法等による製膜は、困難であるために、熱可塑性ポ
リウレタンに溶融張力が高く温度依存性の低い樹脂やブ
ロッキング性を改善する樹脂を混合することにより加工
性を改善することが提案されている。しかし、このよう
な樹脂の添加量の増加により得られたフイルムは、成形
性が改良されるが、当該ウレタン樹脂の持つ本来の透湿
性を損ない、かつ、耐ブロッキング性には未だ改良の余
地を残している。
Further, since the thermoplastic polyurethane elastomer has high tackiness, is easy to block, and has a low melt tension, it is difficult to form a film by a casting method or an inflation method by itself, so that the thermoplastic polyurethane is used. It has been proposed to improve the processability by mixing a resin having a high melt tension and a low temperature dependence or a resin that improves the blocking property. However, the film obtained by increasing the amount of such resin added has improved moldability, but impairs the original moisture permeability of the urethane resin, and there is still room for improvement in blocking resistance. I have left.

【0004】[0004]

【発明が解決しようとする課題】本発明は、かかる従来
技術の有する欠点を解消し、溶融張力の向上、ブロッキ
ングの改善等による成形性を改良したポリエーテル系の
熱可塑性ポリウレタンを用いた透湿性、防水性に富むウ
レタン系エラストマーフイルムであって、機械的強度に
も優れたウレタン系エラストマーフイルムを提供するこ
とを目的とし、特に、おむつ分野において指標とされる
透湿度2000g/m2・24hrs以上、耐水度10
00mmH2O以上の水準をクリアし、伸縮性に優れた
ウレタン系エラストマーフイルムを提供することを目的
とする。
SUMMARY OF THE INVENTION The present invention solves the drawbacks of the prior art and improves the moldability by improving the melt tension, blocking, etc. and uses a polyether-based thermoplastic polyurethane for moisture permeability. , A urethane-based elastomer film that is highly waterproof, with the aim of providing a urethane-based elastomer film that also has excellent mechanical strength, and in particular has a water vapor transmission rate of 2000 g / m 2 · 24 hrs or more, which is an index in the diaper field. , Water resistance 10
It is an object of the present invention to provide a urethane-based elastomer film having a stretchability of more than 00 mmH 2 O and having a high level of elasticity.

【0005】[0005]

【課題を解決するための手段】本発明は、上記目的に鑑
み検討の結果、ポリエーテル系の熱可塑性ポリウレタン
樹脂に、溶融張力が高く温度依存性の低い樹脂と充填剤
とを特定量配合することにより本発明を完成したもので
ある。すなわち、(a)ソフトセグメントがポリエーテ
ルからなる熱可塑性ポリウレタン樹脂75〜95重量%
(b)エチレンープロピレン−ジエン共重合体ゴム5〜
25重量%からなるポリウレタン系樹脂組成物100重
量部に対して(c)充填剤5〜40重量部を添加してな
る熱可塑性エラストマー組成物をフイルム成形してなる
ことを特徴とする透湿性ウレタン系エラストマーフイル
ムに係るものである。
The present invention has been studied in view of the above objects, and as a result, a specific amount of a thermoplastic thermoplastic polyurethane resin is blended with a resin having a high melt tension and a low temperature dependence and a filler. This completes the present invention. That is, (a) 75-95% by weight of a thermoplastic polyurethane resin whose soft segment is composed of polyether.
(B) Ethylene-propylene-diene copolymer rubber 5 to
A moisture-permeable urethane which is formed by film-forming a thermoplastic elastomer composition obtained by adding (c) 5 to 40 parts by weight of filler to 100 parts by weight of a polyurethane resin composition consisting of 25% by weight. System elastomer film.

【0006】以下、本発明を詳細に説明する。本発明に
おける前記(a)熱可塑性ポリウレタン樹脂としては、
ソフトセグメントがポリエーテルからなるポリエーテル
系ポリウレタンエラストマーを使用する。熱可塑性ポリ
ウレタン樹脂は、長鎖グリコール、短鎖グリコール、ジ
イソシアネートの付加重合物であるが、当該ソフトセグ
メントがポリエーテルからなる熱可塑性ポリウレタン樹
脂は、長鎖グリコールとして、ポリテトラメチレングリ
コール(PTMG)、ポリエチレングリコール(PE
G)、ポリプロピレングリコール(PPG)などのポリ
エーテル系化合物、短鎖グリコールとして、エチレング
リコール、1,4−ブタンジオール、1,4−ヘキサン
ジオール、ジイソシアネートとしては、トリレンジイソ
シアネート、4,4´−ジフェニルメタンジイソシアネ
ート、ヘキサメチレンジイソシアネートなどを用い、付
加重合して得られる。
The present invention will be described in detail below. Examples of the (a) thermoplastic polyurethane resin in the present invention include:
A polyether polyurethane elastomer whose soft segment is polyether is used. The thermoplastic polyurethane resin is an addition polymer of a long-chain glycol, a short-chain glycol, and a diisocyanate. The thermoplastic polyurethane resin in which the soft segment is composed of polyether is polytetramethylene glycol (PTMG) as a long-chain glycol, Polyethylene glycol (PE
G), polyether compounds such as polypropylene glycol (PPG), ethylene glycol, 1,4-butanediol, 1,4-hexanediol as the short-chain glycol, and tolylene diisocyanate, 4,4′-as the diisocyanate. It can be obtained by addition polymerization using diphenylmethane diisocyanate, hexamethylene diisocyanate or the like.

【0007】本発明において使用される(b)エチレン
ープロピレン−ジエン共重合体は、エチレン、プロピレ
ン及びジエン化合物を含む共重合体のことである。前記
ジエン化合物としては、エチリデンノルボルネン、1,
4−ヘキサジエン、ジシクロペンタジエンなどがある。
上記エチレン−プロピレン−ジエン共重合体ゴム(EP
DM)は、プロピレンの含有率が10〜80重量%のも
のが好ましい。より好ましくは、15〜70重量%であ
る。当該エチレン−プロピレン−ジエン共重合体の数平
均分子量は40万〜60万が好ましく、密度は0.87
g/cm3 以下が好ましい。さらに、メルトインデッ
クス(190℃,2.16kg荷重)としては、0.1
〜12.0g/10分の範囲内が好ましく、より好まし
くは0.1〜5.0g/10分である。
The (b) ethylene-propylene-diene copolymer used in the present invention is a copolymer containing ethylene, propylene and a diene compound. Examples of the diene compound include ethylidene norbornene, 1,
4-hexadiene, dicyclopentadiene and the like.
The ethylene-propylene-diene copolymer rubber (EP
The DM) preferably has a propylene content of 10 to 80% by weight. More preferably, it is 15 to 70% by weight. The number average molecular weight of the ethylene-propylene-diene copolymer is preferably 400,000 to 600,000, and the density is 0.87.
It is preferably g / cm 3 or less. Furthermore, the melt index (190 ° C., 2.16 kg load) is 0.1
It is preferably in the range of ˜12.0 g / 10 minutes, more preferably 0.1 to 5.0 g / 10 minutes.

【0008】本発明において使用されるポリウレタン系
樹脂組成物における各成分の配合割合は、(a)ソフト
セグメントがポリエーテルからなる熱可塑性ポリウレタ
ン樹脂が75〜95重量%、(b)エチレンープロピレ
ン−ジエン共重合体ゴムが5〜25重量%である。上記
(a)ソフトセグメントがポリエーテルからなる熱可塑
性ポリウレタン樹脂が75重量%未満では、ポリウレタ
ンエラストマーの特性が失われ、透湿度が悪くなり、ま
たポリウレタンの特性である耐摩耗性や機械的強度が低
下する。一方、95重量%を超えると、インフレーショ
ンチューブがブロッキングし易く、両耳スリット後2枚
に剥すことが難しくなる。また、ウレタン樹脂は溶融物
性への温度依存性が高いため、バブルが不安定で、イン
フレーション法による製膜が困難となる。(b)エチレ
ンープロピレン−ジエン共重合体ゴムが5重量%未満で
は、インフレーションチューブがブロッキングし易く、
両耳スリット後2枚に剥すことが難しくなり、フイルム
の製膜における安定性が不十分となる。一方、25重量
%を超えると、伸縮柔軟性は維持されるが、製品の透湿
度が著しく低下する。
The blending ratio of each component in the polyurethane resin composition used in the present invention is as follows: (a) 75 to 95% by weight of a thermoplastic polyurethane resin in which the soft segment is composed of polyether, (b) ethylene-propylene- The diene copolymer rubber is 5 to 25% by weight. When the content of the thermoplastic polyurethane resin (a) in which the soft segment is composed of polyether is less than 75% by weight, the properties of the polyurethane elastomer are lost, the moisture permeability is deteriorated, and the properties of the polyurethane such as abrasion resistance and mechanical strength are deteriorated. descend. On the other hand, if it exceeds 95% by weight, the inflation tube is likely to be blocked, and it becomes difficult to peel it off into two pieces after slitting both ears. Further, since the urethane resin has a high temperature dependency on the melt property, the bubbles are unstable and it becomes difficult to form a film by the inflation method. (B) If the ethylene-propylene-diene copolymer rubber is less than 5% by weight, the inflation tube tends to be blocked,
It becomes difficult to peel it into two pieces after slitting both ears, and the stability in film formation of the film becomes insufficient. On the other hand, if it exceeds 25% by weight, the flexibility of stretching is maintained, but the moisture permeability of the product is significantly lowered.

【0009】上記ポリウレタン系樹脂組成物において
は、低密度ポリエチレン系樹脂を配合することにより、
より一層溶融張力の向上、ブロッキングの改善等による
成形性を改良できる。当該低密度ポリエチレン系樹脂と
しては、高圧法によるエチレンの単独重合体、線状低密
度ポリエチレンまたはエチレンを主成分とし20重量%
以下のビニル系化合物等との共重合体例えばエチレンー
酢酸ビニル共重合体、エチレンーアクリル酸エチル共重
合体等があげられる。当該低密度ポリエチレン系樹脂の
密度は、0.935g/cm3以下のものが好ましく、
またメルトインデックス(MI、190℃、荷重2,1
6kg)が0.05〜20g/10分のものが好まし
い。低密度ポリエチレン系樹脂を配合する場合、(b)
エチレンープロピレン−ジエン共重合体ゴムの40重量
%までとすることが好ましい。低密度ポリエチレン系樹
脂の配合比率が、40重量%以上では、製品の透湿度が
損なわれ、また、伸縮柔軟性が不足する。
In the above polyurethane resin composition, by blending a low density polyethylene resin,
The moldability can be improved by further improving the melt tension and blocking. As the low-density polyethylene-based resin, a homopolymer of ethylene by a high-pressure method, linear low-density polyethylene or 20% by weight containing ethylene as a main component
The following copolymers with vinyl compounds and the like, for example, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer and the like can be mentioned. The density of the low density polyethylene resin is preferably 0.935 g / cm 3 or less,
Also, melt index (MI, 190 ° C, load 2, 1
6 kg) is preferably 0.05 to 20 g / 10 minutes. When blending low density polyethylene resin, (b)
It is preferably up to 40% by weight of the ethylene-propylene-diene copolymer rubber. If the blending ratio of the low-density polyethylene-based resin is 40% by weight or more, the moisture permeability of the product will be impaired, and the flexibility of stretching will be insufficient.

【0010】本発明における熱可塑性エラストマー組成
物には、(c)充填剤が添加される。(c)充填剤とし
ては、タルク、炭酸カルシウム、セッコウ、カ−ボンブ
ラック、クレ−、カオリン、シリカ、ケイソウ土、炭酸
マグネシウム、炭酸バリウム、硫酸マグネシウム、硫酸
バリウム、硫酸カルシウム、リン酸カルシウム、水酸化
アルミニウム、酸化亜鉛、水酸化マグネシウム、酸化カ
ルシウム、酸化マグネシウム、酸化チタン、アルミナ、
マイカ、シラスバル−ン、ゼオライト、珪酸白土、セメ
ント、シリカフュ−ム、雲母粉、ナイロンパウダー等の
ブロッキング防止効果のあるものを使用することができ
るが、タルク、酸化チタン、炭酸カルシウム、シリカ等
が特に好ましい。これらの充填剤は、単独であるいは組
み合わせて使用することができる。また、充填剤は、表
面処理を施したものを用いてもよい。上記充填剤の添加
量は、上記ポリウレタン系樹脂組成物100重量部に対
して5〜40重量部である。充填剤の添加量が5重量部
未満では、フイルムのMD/TD方向の物性バランスは
良好であるが、耐ブロッキング性が改善されない。ま
た、40重量部を超えると、耐ブロッキング性は改善さ
れるが、強度が高くなり、柔軟性が損なわれる。
A filler (c) is added to the thermoplastic elastomer composition of the present invention. Examples of the filler (c) include talc, calcium carbonate, gypsum, carbon black, clay, kaolin, silica, diatomaceous earth, magnesium carbonate, barium carbonate, magnesium sulfate, barium sulfate, calcium sulfate, calcium phosphate, and aluminum hydroxide. , Zinc oxide, magnesium hydroxide, calcium oxide, magnesium oxide, titanium oxide, alumina,
Mica, silas balun, zeolite, silicate clay, cement, silica fume, mica powder, nylon powder and the like having an anti-blocking effect can be used, but talc, titanium oxide, calcium carbonate, silica and the like are particularly preferable. preferable. These fillers can be used alone or in combination. The filler may be surface-treated. The amount of the filler added is 5 to 40 parts by weight based on 100 parts by weight of the polyurethane resin composition. When the amount of the filler added is less than 5 parts by weight, the physical property balance in the MD / TD direction of the film is good, but the blocking resistance is not improved. If it exceeds 40 parts by weight, blocking resistance is improved, but strength is increased and flexibility is impaired.

【0011】上記熱可塑性エラストマー組成物には、必
要に応じて、酸化防止剤、紫外線吸収剤、着色剤等を適
宜配合することができる。
If necessary, an antioxidant, an ultraviolet absorber, a colorant and the like can be added to the above thermoplastic elastomer composition.

【0012】本発明では、上記熱可塑性エラストマー組
成物を、二軸押出機等を用いて溶融混練し、フイルムに
成形する。当該組成物からフイルムを製造する方法は、
通常ポリオレフインフイルムを成形する公知の方法であ
るTーダイ押出機によるフラットなフイルムとして成形
することができるが、インフレーシヨン法によるチユー
ブ状のフイルムとして成形する空冷インフレーシヨン法
が好ましい。空冷インフレーシヨン法において、薄膜化
と成形の高速化に必要なバブルを安定させ、熱可塑性ポ
リウレタン樹脂の特性を損うことなくブロッキング性を
低減できる。当該空冷法によるインフレーシヨン成形法
では、薄膜化と成形の高速化に必要なバブルを安定さ
せ、熱可塑性ポリウレタン樹脂の特性を損うことなくブ
ロッキング性を低減するためには、樹脂温度180〜2
20℃で、ブロー比を2.0〜5.0の範囲で行うのが
好ましい。このようなフイルムの製造方法等については
特開平3−128945号公報に開示の事項が適用でき
る。フイルムの厚さは、各種用途により適宜選択される
が、薄膜化と成形の高速化に必要なバブルを安定させ、
熱可塑性ポリウレタン樹脂の透湿度をはじめとする特性
を損うことなくブロッキング性を低減するためには、通
常、25〜40μm程度の範囲で成形することが好まし
い。
In the present invention, the thermoplastic elastomer composition is melt-kneaded by using a twin-screw extruder or the like to form a film. The method for producing a film from the composition,
Although it can be usually formed into a flat film by a T-die extruder, which is a known method for forming a polyolefin film, an air-cooled inflation method of forming a tube-shaped film by an inflation method is preferable. In the air-cooled inflation method, it is possible to stabilize the bubbles required for thinning and high-speed molding, and to reduce the blocking property without deteriorating the characteristics of the thermoplastic polyurethane resin. In the inflation molding method using the air-cooling method, in order to stabilize the bubbles necessary for thinning the film and speeding up the molding, and to reduce the blocking property without deteriorating the characteristics of the thermoplastic polyurethane resin, a resin temperature of 180 to Two
It is preferable to carry out at 20 ° C. and a blow ratio of 2.0 to 5.0. The matters disclosed in JP-A-3-128945 can be applied to such a film manufacturing method. The thickness of the film is appropriately selected according to various uses, but it stabilizes the bubbles required for thinning and high-speed molding,
In order to reduce the blocking property without deteriorating the characteristics such as moisture permeability of the thermoplastic polyurethane resin, it is usually preferable to mold the thermoplastic polyurethane resin in the range of about 25 to 40 μm.

【0013】[0013]

【実施例】次に、本発明の実施例を示す。なお、実施例
及び比較例における試験方法は次の通りである。 (1)透湿度;JIS Z0208に準拠。 (2)耐水度;JIS L1092に準拠。 (3)破断時強度;JIS L1096に準拠。 (4)破断時伸度:JIS L1096に準拠。 (5)50%2サイクル歪;JIS L1096に準
拠。 (6)製膜性;◎・・・バブルが全く安定してブロッキ
ング全くなし、○・・・バブルが安定してブロッキング
なし、△・・・バブルが不安定でブロッキングあり、X
・・・製膜不可。
EXAMPLES Next, examples of the present invention will be shown. The test methods in Examples and Comparative Examples are as follows. (1) Water vapor transmission rate; conforms to JIS Z0208. (2) Water resistance: According to JIS L1092. (3) Strength at break: According to JIS L1096. (4) Elongation at break: According to JIS L1096. (5) 50% 2-cycle strain; conforming to JIS L1096. (6) Film-forming property: ◎ ... Bubbles are stable and do not block at all, ○ ... Bubbles are stable and do not block, Δ ... Bubbles are unstable and block, X
... No film formation.

【0014】実施例1〜3.ソフトセグメントがポリエ
ーテルからなる熱可塑性ポリウレタン樹脂(大日精化工
業(株)製商品名レザミンPー210)とエチレンープ
ロピレンージエン共重合体(数平均分子量45万、密度
0.87g/cm、MI=0.1g/10分、プロピ
レン含有量27wt%)および、高圧法低密度ポリエチ
レン(密度0.935g/cm、MI=0.8g/1
0分)とからなる表1に示す配合比の組成物100重量
部に対して、ステアリン酸処理炭酸カルシウム(平均粒
径2μm)30重量部を添加してなる組成物を、180
℃にて二軸混練機により溶融混練し、空冷インフレ−シ
ョン法により下記の条件で30μm厚、40μm厚およ
び30μm厚のフイルムを製膜して、それぞれ実施例
1、2、3とした。 ダイ径・・・150mm、 ブロ−比・・・3.5, 押出機のシリンダ温度・・・190℃ ダイ出口の樹脂温度・・・・195℃、 ダイ出口の樹脂圧力・・・・200kg/cm2、 押出し量・・・35〜45kg/hr、 引取速度・・10m/分、
Examples 1-3. Thermoplastic polyurethane resin whose soft segment is composed of polyether (trade name: Rezamin P-210 manufactured by Dainichiseika Kogyo Co., Ltd.) and ethylene-propylene-diene copolymer (number average molecular weight 450,000, density 0.87 g / cm 3 , MI = 0.1 g / 10 min, propylene content 27 wt%) and high-pressure low-density polyethylene (density 0.935 g / cm 3 , MI = 0.8 g / 1
The composition obtained by adding 30 parts by weight of stearic acid-treated calcium carbonate (average particle size 2 μm) to 100 parts by weight of the composition having the compounding ratio shown in Table 1 is 180 minutes.
The film was melt-kneaded with a biaxial kneader at 0 ° C., and films having a thickness of 30 μm, a thickness of 40 μm and a thickness of 30 μm were formed into films by the air-cooled inflation method under the following conditions, to give Examples 1, 2 and 3, respectively. Die diameter: 150 mm, Blow ratio: 3.5, Cylinder temperature of extruder: 190 ° C Resin temperature at die outlet: 195 ° C, Resin pressure at die outlet: 200 kg / cm 2 , extrusion rate ... 35-45 kg / hr, take-up speed ... 10 m / min,

【0015】得られたエラストマーフィルムについて、
透湿度、耐水度、破断時強度、破断時伸度、および50
%2サイクル歪を測定した。その結果を表1に示す。
Regarding the obtained elastomer film,
Moisture vapor transmission rate, water resistance, strength at break, elongation at break, and 50
% 2 cycle strain was measured. The results are shown in Table 1.

【0016】比較例1.実施例1〜3で使用のソフトセ
グメントがポリエーテルからなる熱可塑性ポリウレタン
樹脂50wt%、エチレンープロピレンージエン共重合
体30wt%および高圧法低密度ポリエチレン20wt
%とからなる組成物を、実施例1と同様にして、180
℃にて二軸混練機により溶融混練し、空冷インフレ−シ
ョン法によりフイルムを製膜した。成膜性、機械的物性
は良好であるが、熱可塑性ポリウレタン樹脂の量が少な
いため、透湿性が阻害されてしまった。
Comparative Example 1. 50 wt% of the thermoplastic polyurethane resin whose soft segment used in Examples 1 to 3 is polyether, 30 wt% of ethylene-propylene-diene copolymer, and 20 wt% of high-pressure low-density polyethylene.
% In the same manner as in Example 1.
The film was melted and kneaded by a biaxial kneader at ℃, and a film was formed by an air-cooled inflation method. The film-forming property and the mechanical properties are good, but the moisture permeability is impaired because the amount of the thermoplastic polyurethane resin is small.

【0017】比較例2.実施例1において、ステアリン
酸処理炭酸カルシウムを配合しなかったことおよび膜厚
を60μmとした以外は同様にしてフイルムを製膜し
た。製膜時、空冷インフレ−ション法で膨らませた後に
ニップロールで押圧し、チューブを折畳んだ後に両耳を
トリミングして2枚に分けようとしたが、ブロッキング
して剥れなかった。尚、表1における透湿度および耐水
度の測定値は、二枚重ねのものについての値である。ま
た、製膜終了後に巻取機(ワインダー)からフイルムを
繰り出すのも困難な個所も見られた。その他の機械物性
については測定できなかった。
Comparative Example 2. A film was formed in the same manner as in Example 1 except that the stearic acid-treated calcium carbonate was not added and the film thickness was changed to 60 μm. During film formation, the film was inflated by an air-cooled inflation method and then pressed with a nip roll to fold the tube and then trimmed both ears to divide it into two pieces, but they were blocked and did not come off. The measured values of the water vapor transmission rate and the water resistance in Table 1 are the values for the two-layer stack. Moreover, it was found that it was difficult to feed the film from the winder after the film formation. Other mechanical properties could not be measured.

【0018】比較例3.実施例1において、エチレンー
プロピレンージエン共重合体を配合しなかった以外は同
様にしてフイルムを製膜しようとしたが、溶融張力が低
く、製膜が不可能であった。
Comparative Example 3. An attempt was made to form a film in the same manner as in Example 1 except that the ethylene-propylene-diene copolymer was not blended, but the melt tension was low and film formation was impossible.

【0019】[0019]

【表1】 [Table 1]

【0020】[0020]

【発明の効果】以上本発明によれば、溶融張力の向上、
ブロッキングの改善等による成形性を改良し、低コスト
で生産性のよいインフレーション法によるポリエーテル
系の熱可塑性ポリウレタンを用いた透湿性、防水性に富
み、機械的強度にも優れたウレタン系エラストマーフイ
ルムを提供することができる。特に、おむつ分野におい
て指標とされる透湿度2000g/m2・24hrs以
上、耐水度1000mmH2O以上の水準をクリアし、
伸縮性に優れたウレタン系エラストマーフイルムを提供
することができた。
As described above, according to the present invention, the melt tension is improved,
A urethane elastomer film that has improved mechanical properties due to improved blocking properties, and uses a thermoplastic thermoplastic polyurethane based on an inflation method with low cost and high productivity, which has excellent moisture permeability and waterproof properties as well as excellent mechanical strength. Can be provided. In particular, it has cleared the water vapor permeability of 2000 g / m 2 · 24 hrs or more and the water resistance of 1000 mmH 2 O or more, which are indicators in the diaper field,
It was possible to provide a urethane-based elastomer film having excellent stretchability.

───────────────────────────────────────────────────── フロントページの続き (51)Int.Cl.6 識別記号 庁内整理番号 FI 技術表示箇所 B29K 75:00 ─────────────────────────────────────────────────── ─── Continuation of the front page (51) Int.Cl. 6 Identification code Internal reference number FI technical display location B29K 75:00

Claims (3)

【特許請求の範囲】[Claims] 【請求項1】(a)ソフトセグメントがポリエーテルか
らなる熱可塑性ポリウレタン樹脂75〜95重量%
(b)エチレンープロピレン−ジエン共重合体ゴム5〜
25重量%からなるポリウレタン系樹脂組成物100重
量部に対して(c)充填剤5〜40重量部を添加してな
る熱可塑性エラストマー組成物をフイルム成形してなる
ことを特徴とする透湿性ウレタン系エラストマーフイル
ム。
1. A thermoplastic polyurethane resin comprising: (a) a soft segment composed of polyether;
(B) Ethylene-propylene-diene copolymer rubber 5 to
A moisture-permeable urethane which is formed by film-forming a thermoplastic elastomer composition obtained by adding (c) 5 to 40 parts by weight of filler to 100 parts by weight of a polyurethane resin composition consisting of 25% by weight. Type elastomer film.
【請求項2】ポリウレタン系樹脂組成物が、低密度ポリ
エチレン系樹脂を含有してなることを特徴とする、請求
項1に記載の透湿性ウレタン系エラストマーフイルム。
2. The moisture-permeable urethane elastomer film according to claim 1, wherein the polyurethane resin composition contains a low density polyethylene resin.
【請求項3】フイルム成形が、インフレーション法によ
り行われることを特徴とする、請求項1または2に記載
の透湿性ウレタン系エラストマーフイルム。
3. The moisture-permeable urethane elastomer film according to claim 1, wherein the film is formed by an inflation method.
JP21521094A 1994-08-18 1994-08-18 Moisture-permeable urethane-based elastomer film Pending JPH0859981A (en)