JP6397644B2 - Surface protection film - Google Patents

Surface protection film Download PDF

Info

Publication number
JP6397644B2
JP6397644B2 JP2014069552A JP2014069552A JP6397644B2 JP 6397644 B2 JP6397644 B2 JP 6397644B2 JP 2014069552 A JP2014069552 A JP 2014069552A JP 2014069552 A JP2014069552 A JP 2014069552A JP 6397644 B2 JP6397644 B2 JP 6397644B2
Authority
JP
Japan
Prior art keywords
protective film
intermediate layer
surface protective
sensitive adhesive
pressure
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2014069552A
Other languages
Japanese (ja)
Other versions
JP2015189909A (en
Inventor
文音 下村
文音 下村
輝 中田
輝 中田
豊嶋 克典
克典 豊嶋
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sekisui Chemical Co Ltd
Original Assignee
Sekisui Chemical Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sekisui Chemical Co Ltd filed Critical Sekisui Chemical Co Ltd
Priority to JP2014069552A priority Critical patent/JP6397644B2/en
Publication of JP2015189909A publication Critical patent/JP2015189909A/en
Application granted granted Critical
Publication of JP6397644B2 publication Critical patent/JP6397644B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は、ポリオレフィン系樹脂により形成された基材上に、中間層及び粘着剤層がこの順で積層されている表面保護フィルムに関する。   The present invention relates to a surface protective film in which an intermediate layer and an adhesive layer are laminated in this order on a substrate formed of a polyolefin-based resin.

従来、合成樹脂板、化粧合板及び金属板等の表面に対して、塵の付着や傷付きを防止する目的で、表面保護フィルムが用いられている。   Conventionally, surface protective films have been used for the purpose of preventing dust adhesion and scratches on the surfaces of synthetic resin plates, decorative plywood, metal plates and the like.

例えば、下記の特許文献1には、熱可塑性樹脂により形成された基材層上に、中間層及び粘着剤層がこの順に積層されている表面保護フィルムが開示されている。上記中間層は、上記基材層を構成する成分と上記粘着剤層を構成する成分とを含む樹脂組成物により形成されている。上記中間層の厚みは7〜20μmである。   For example, Patent Document 1 below discloses a surface protective film in which an intermediate layer and an adhesive layer are laminated in this order on a base material layer formed of a thermoplastic resin. The said intermediate | middle layer is formed with the resin composition containing the component which comprises the said base material layer, and the component which comprises the said adhesive layer. The intermediate layer has a thickness of 7 to 20 μm.

また、特許文献1では、上記中間層を構成する材料に、従来廃棄されていた表面保護フィルムの「耳」を、回収原料として使用できることが記載されている。さらに、特許文献1では、上記中間層として「耳」を用いる場合には、この樹脂が一度共押出成形されたときに受けた熱履歴と再度行われる共押出成形時に受ける熱履歴とによって、中間層が厚すぎると表面保護フィルムにフィッシュアイが生じ易くなることがあり、剥離力によって中間層が凝集破壊され易くなることが記載されている。このような理由から、特許文献1では、上記中間層の厚みは20μm以下に限定されている。   Further, Patent Document 1 describes that the “ear” of the surface protection film that has been conventionally discarded can be used as a collected raw material for the material constituting the intermediate layer. Further, in Patent Document 1, when “ears” are used as the intermediate layer, an intermediate between the heat history received when the resin is once co-extruded and the heat history received during the co-extrusion performed again. It is described that when the layer is too thick, fish eyes are likely to be generated in the surface protective film, and the intermediate layer is likely to be cohesively broken by the peeling force. For these reasons, in Patent Document 1, the thickness of the intermediate layer is limited to 20 μm or less.

特許第3088190号公報Japanese Patent No. 3088190

従来の表面保護フィルムでは、ロール状態の表面保護フィルムを良好に巻き出したり、表面保護フィルムを被着体に良好に貼り合わせたりするためには、巻き出し時又は貼り合わせ時に、表面保護フィルムを弱い力で引っ張らなければならないことがある。このため、表面保護フィルムを取り扱う際の作業効率が低いという問題がある。また、表面保護フィルムを被着体に貼り合わせた後に、貼り合わせ品がカールすることがある。   In the conventional surface protection film, in order to unwind the surface protection film in a roll state or to bond the surface protection film to the adherend well, the surface protection film is used at the time of unwinding or bonding. You may have to pull with a weak force. For this reason, there exists a problem that the working efficiency at the time of handling a surface protection film is low. Further, the bonded product may be curled after the surface protective film is bonded to the adherend.

また、特許文献1に記載の表面保護フィルムでは、中間層に、従来廃棄されていた表面保護フィルムの「耳」が回収原料として使用されている。このため、表面保護フィルムの原材料費を抑えることができる。   Further, in the surface protective film described in Patent Document 1, the “ear” of the surface protective film that has been conventionally discarded is used as a collected raw material for the intermediate layer. For this reason, the raw material cost of a surface protection film can be held down.

一方で、中間層と粘着剤層とを備える表面保護フィルムでは、中間層と粘着剤層との層間強度が高く、中間層と粘着剤層との層間で剥離が生じないことが求められている。例えば、表面保護フィルムを被着体に貼り合わせた後、表面保護フィルムを剥離したときに、被着体に糊残りが生じないことが求められている。特許文献1に記載の表面保護フィルムでは、中間層と粘着剤層との層間強度はある程度高くなるものの、この層間強度をより一層高めることが求められている。   On the other hand, in a surface protective film provided with an intermediate layer and an adhesive layer, the interlayer strength between the intermediate layer and the adhesive layer is high, and it is required that no peeling occurs between the intermediate layer and the adhesive layer. . For example, when the surface protective film is bonded to the adherend and then peeled off, it is required that no adhesive residue is generated on the adherend. In the surface protective film described in Patent Document 1, although the interlayer strength between the intermediate layer and the pressure-sensitive adhesive layer is increased to some extent, it is required to further increase the interlayer strength.

本発明の目的は、中間層と粘着剤層との層間強度を高めることができ、かつ、取扱い性に優れている表面保護フィルムを提供することである。   An object of the present invention is to provide a surface protective film that can increase the interlayer strength between the intermediate layer and the pressure-sensitive adhesive layer and is excellent in handleability.

本発明の広い局面によれば、基材と、上記基材の一方の表面に積層された中間層と、上記中間層の上記基材側とは反対の表面に積層された粘着剤層とを備え、上記基材が、ポリオレフィン系樹脂により形成されており、上記粘着剤層が、合成ゴム系粘着剤により形成されており、上記中間層が、ポリオレフィン系樹脂85重量%以上、97重量%以下と、合成ゴム系粘着剤3重量%以上、15重量%以下とを含む、表面保護フィルムが提供される。   According to a wide aspect of the present invention, a base material, an intermediate layer laminated on one surface of the base material, and an adhesive layer laminated on the surface of the intermediate layer opposite to the base material side The base material is formed of a polyolefin-based resin, the adhesive layer is formed of a synthetic rubber-based adhesive, and the intermediate layer is 85% by weight or more and 97% by weight or less of the polyolefin resin. And a synthetic rubber-based pressure sensitive adhesive 3 wt% or more and 15 wt% or less.

本発明に係る表面保護フィルムのある特定の局面では、上記中間層の厚みが、20μmを超え、60μm以下である。   On the specific situation with the surface protection film which concerns on this invention, the thickness of the said intermediate | middle layer exceeds 20 micrometers and is 60 micrometers or less.

本発明に係る表面保護フィルムのある特定の局面では、上記中間層に含まれる上記合成ゴム系粘着剤が、合成ゴムを含む。上記中間層に含まれる上記合成ゴム系粘着剤は、合成ゴムと、粘着付与樹脂とを含んでいてもよい。   On the specific situation with the surface protection film which concerns on this invention, the said synthetic rubber adhesive contained in the said intermediate | middle layer contains a synthetic rubber. The synthetic rubber adhesive contained in the intermediate layer may contain a synthetic rubber and a tackifier resin.

本発明に係る表面保護フィルムのある特定の局面では、上記中間層に含まれる上記合成ゴム系粘着剤において、上記合成ゴム100重量部に対する上記粘着付与樹脂の含有量が、5重量部以上、50重量部以下である。   On the specific situation with the surface protection film which concerns on this invention, in the said synthetic rubber-type adhesive contained in the said intermediate | middle layer, content of the said tackifying resin with respect to 100 weight part of said synthetic rubbers is 5 weight part or more, 50 Less than parts by weight.

上記合成ゴムは、スチレン系エラストマーであることが好ましい。上記スチレン系エラストマーが、水素添加されたスチレン系エラストマーであることが好ましい。上記水素添加されたスチレン系エラストマーが、スチレン−エチレン−ブチレン−スチレン共重合体であることが好ましい。   The synthetic rubber is preferably a styrene elastomer. The styrene elastomer is preferably a hydrogenated styrene elastomer. The hydrogenated styrene elastomer is preferably a styrene-ethylene-butylene-styrene copolymer.

本発明に係る表面保護フィルムは、基材と中間層と粘着剤層とがこの順で積層されており、上記基材が、ポリオレフィン系樹脂により形成されており、上記粘着剤層が、合成ゴム系粘着剤により形成されており、上記中間層が、ポリオレフィン系樹脂85重量%以上、97重量%以下と、合成ゴム系粘着剤3重量%以上、15重量%以下とを含むので、中間層と粘着剤層との層間強度を高めることができ、かつ、表面保護フィルムの取扱い性を高めることができる。   In the surface protective film according to the present invention, a base material, an intermediate layer, and an adhesive layer are laminated in this order, the base material is formed of a polyolefin-based resin, and the adhesive layer is a synthetic rubber. Since the intermediate layer includes 85% by weight or more and 97% by weight or less of the polyolefin resin and 3% by weight or more and 15% by weight or less of the synthetic rubber adhesive, The interlayer strength with the pressure-sensitive adhesive layer can be increased, and the handleability of the surface protective film can be increased.

以下、本発明の詳細を説明する。   Details of the present invention will be described below.

[表面保護フィルム]
本発明に係る表面保護フィルムは、基材と、中間層と、粘着剤層とを備える。上記中間層は、上記基材の一方の表面に積層されている。上記粘着剤層は、上記中間層の上記基材側とは反対の表面に積層されている。上記中間層は、上記基材と上記粘着剤層との間に配置されている。従って、本発明に係る表面保護フィルムは、上記基材と上記中間層と上記粘着剤層とがこの順で積層された構造を有する。
[Surface protection film]
The surface protective film according to the present invention includes a base material, an intermediate layer, and an adhesive layer. The intermediate layer is laminated on one surface of the base material. The said adhesive layer is laminated | stacked on the surface on the opposite side to the said base material side of the said intermediate | middle layer. The intermediate layer is disposed between the base material and the pressure-sensitive adhesive layer. Therefore, the surface protective film according to the present invention has a structure in which the substrate, the intermediate layer, and the pressure-sensitive adhesive layer are laminated in this order.

上記基材は、ポリオレフィン系樹脂により形成されている。上記粘着剤層は、合成ゴム系粘着剤により形成されている。上記中間層は、ポリオレフィン系樹脂と合成ゴム系粘着剤とにより形成されている。上記中間層100重量%中、上記ポリオレフィン系樹脂の含有量は85重量%以上、97重量%以下であり、上記合成ゴム系粘着剤の含有量は3重量%以上、15重量%以下である。   The base material is formed of a polyolefin resin. The pressure-sensitive adhesive layer is formed of a synthetic rubber pressure-sensitive adhesive. The intermediate layer is formed of a polyolefin resin and a synthetic rubber adhesive. In 100% by weight of the intermediate layer, the content of the polyolefin-based resin is 85% by weight or more and 97% by weight or less, and the content of the synthetic rubber-based pressure-sensitive adhesive is 3% by weight or more and 15% by weight or less.

本発明では、上記の構成が採用されているので、中間層と粘着剤層との層間強度を高めることができ、中間層と粘着剤層との剥離を抑えることができる。また、中間層と粘着剤層との層間強度を高めることで、表面保護フィルムを被着体から剥離した後に、被着体に糊残りが生じ難くなる。従って、本発明に係る表面保護フィルムは、信頼性に優れている。   In this invention, since said structure is employ | adopted, the interlayer strength of an intermediate | middle layer and an adhesive layer can be raised, and peeling with an intermediate | middle layer and an adhesive layer can be suppressed. Further, by increasing the interlayer strength between the intermediate layer and the pressure-sensitive adhesive layer, it is difficult for adhesive residue to occur on the adherend after the surface protective film is peeled off from the adherend. Therefore, the surface protective film according to the present invention is excellent in reliability.

さらに、本発明では、上記の構成が採用されているので、表面保護フィルムの取扱い性を高めることができる。ロール状態の表面保護フィルムを良好に巻き出すことができ、表面保護フィルムを被着体に良好に貼り合わせることができる。ロール状態の表面保護フィルムを巻き出す際や、表面保護フィルムを被着体に貼り合わせる際に、表面保護フィルムにある程度強い引っ張り応力が付与されても、良好に巻き出したり、良好に貼り合わせを行ったりすることができる。このため、表面保護フィルムを取り扱う際の作業効率が高くなる。   Furthermore, in the present invention, since the above-described configuration is adopted, the handleability of the surface protective film can be improved. The surface protective film in a roll state can be unwound well, and the surface protective film can be satisfactorily bonded to the adherend. When unrolling a surface protection film in a roll state or pasting the surface protection film to an adherend, even if a certain amount of strong tensile stress is applied to the surface protection film, the surface protection film can be unwound well or stuck together Can go. For this reason, the work efficiency at the time of handling a surface protection film becomes high.

さらに、本発明では、上記の構成が採用されているので、表面保護フィルムが比較的高温に晒されたときに、表面保護フィルムが収縮し難い。このため、表面保護フィルムを被着体に貼り合わせた後に、貼り合わせ品が比較的高温に晒されても、貼り合わせ品がカールし難くなり、結果として被着体もカールし難くなり、表面保護フィルムが被着体から剥離し難くなる。   Furthermore, in the present invention, since the above configuration is employed, the surface protective film is unlikely to shrink when the surface protective film is exposed to a relatively high temperature. For this reason, even after the surface protective film is bonded to the adherend, even if the bonded product is exposed to a relatively high temperature, the bonded product is difficult to curl. As a result, the adherend is also difficult to curl, The protective film is difficult to peel from the adherend.

さらに、本願発明に係る表面保護フィルムでは、基材と中間層との双方に、ポリオレフィン系樹脂が用いられており、中間層との粘着剤層との双方に、合成ゴム系粘着剤が用いられている。本願発明に係る表面保護フィルムでは、中間層に、ポリオレフィン系樹脂と合成ゴム系粘着剤とが用いられており、基材と粘着剤層とに全体として、ポリオレフィン系樹脂と合成ゴム系粘着剤とが用いられている。このため、本発明では、ポリオレフィン系樹脂と合成ゴム系粘着剤とが用いられており、かつ、基材と粘着剤層とを備える表面保護フィルムの一部又は全部や、ポリオレフィン系樹脂と合成ゴム系粘着剤とが用いられており、かつ、基材と中間層と粘着剤層とを備える表面保護フィルムの一部又は全部を、上記中間層の回収原料として用いることができる。回収原料を用いれば、本発明に係る表面保護フィルムは、安価に製造することができる。また、回収原料を用いれば、環境負荷を低減することができる。   Furthermore, in the surface protective film according to the present invention, a polyolefin resin is used for both the base material and the intermediate layer, and a synthetic rubber adhesive is used for both the adhesive layer and the intermediate layer. ing. In the surface protective film according to the present invention, a polyolefin resin and a synthetic rubber pressure sensitive adhesive are used for the intermediate layer, and the polyolefin resin and the synthetic rubber pressure sensitive adhesive as a whole are formed on the base material and the pressure sensitive adhesive layer. Is used. For this reason, in the present invention, a polyolefin resin and a synthetic rubber adhesive are used, and a part or all of a surface protective film provided with a base material and an adhesive layer, or a polyolefin resin and a synthetic rubber. In addition, a part or all of the surface protective film including the base material, the intermediate layer, and the pressure-sensitive adhesive layer can be used as the recovered raw material for the intermediate layer. If the recovered raw material is used, the surface protective film according to the present invention can be manufactured at a low cost. Moreover, if the recovered raw material is used, the environmental load can be reduced.

以下、表面保護フィルムを構成する各層の詳細等を説明する。   Hereinafter, details of each layer constituting the surface protection film will be described.

(中間層)
上記中間層は、ポリオレフィン系樹脂と、合成ゴム系粘着剤とを含む。上記中間層を形成するための組成物は、ポリオレフィン系樹脂と、合成ゴム系粘着剤とを含む。上記中間層は、ポリオレフィン系樹脂と、合成ゴム系粘着剤とにより形成されている。
(Middle layer)
The intermediate layer includes a polyolefin resin and a synthetic rubber adhesive. The composition for forming the said intermediate | middle layer contains polyolefin resin and a synthetic rubber adhesive. The intermediate layer is formed of a polyolefin resin and a synthetic rubber adhesive.

上記中間層において、上記ポリオレフィン系樹脂の含有量は85重量%以上、97重量%以下であり、上記合成ゴム系粘着剤の含有量は3重量%以上、15重量%以下である。上記ポリオレフィン系樹脂の含有量が上記下限以上及び上記合成ゴム系粘着剤の含有量が上記上限以下であると、表面保護フィルムの取扱い性が高くなり、貼り合わせ品のカールが生じ難くなり、更に表面保護フィルムの高温での寸法安定性が高くなる。上記ポリオレフィン系樹脂の含有量が上記上限以下及び上記合成ゴム系粘着剤の含有量が上記下限以上であると、中間層と粘着剤層との層間強度が高くなる。   In the intermediate layer, the content of the polyolefin resin is 85 wt% or more and 97 wt% or less, and the content of the synthetic rubber pressure-sensitive adhesive is 3 wt% or more and 15 wt% or less. When the content of the polyolefin-based resin is not less than the above lower limit and the content of the synthetic rubber-based pressure-sensitive adhesive is not more than the above upper limit, the handleability of the surface protection film is increased, and the curling of the bonded product is less likely to occur. The dimensional stability at a high temperature of the surface protective film is increased. When the content of the polyolefin-based resin is not more than the above upper limit and the content of the synthetic rubber-based adhesive is not less than the above lower limit, the interlayer strength between the intermediate layer and the adhesive layer is increased.

表面保護フィルムの取扱い性を効果的に高くし、貼り合わせ品のカールをより一層生じ難くする観点からは、上記中間層において、上記ポリオレフィン系樹脂の含有量は好ましくは86.0重量%以上、上記合成ゴム系粘着剤の含有量は好ましくは14.0重量%以下であり、上記ポリオレフィン系樹脂の含有量はより好ましくは87.0重量%以上、上記合成ゴム系粘着剤の含有量はより好ましくは13.0重量%以下である。中間層と粘着剤層との層間強度をより一層高める観点からは、上記中間層において、上記ポリオレフィン系樹脂の含有量は好ましくは96重量%以下、上記合成ゴム系粘着剤の含有量は好ましくは4重量%以上であり、上記ポリオレフィン系樹脂の含有量はより好ましくは95.0重量%以下、上記合成ゴム系粘着剤の含有量はより好ましくは5.0重量%以上である。   From the viewpoint of effectively increasing the handleability of the surface protective film and further reducing the curling of the bonded product, the content of the polyolefin resin in the intermediate layer is preferably 86.0% by weight or more, The content of the synthetic rubber-based adhesive is preferably 14.0% by weight or less, the content of the polyolefin-based resin is more preferably 87.0% by weight or more, and the content of the synthetic rubber-based adhesive is more Preferably it is 13.0 weight% or less. From the viewpoint of further increasing the interlayer strength between the intermediate layer and the pressure-sensitive adhesive layer, the content of the polyolefin-based resin in the intermediate layer is preferably 96% by weight or less, and the content of the synthetic rubber-based pressure-sensitive adhesive is preferably The content of the polyolefin-based resin is more preferably 95.0% by weight or less, and the content of the synthetic rubber-based pressure-sensitive adhesive is more preferably 5.0% by weight or more.

ポリオレフィン系樹脂:
上記中間層に含まれるポリオレフィン系樹脂は、上記基材に含まれるポリオレフィン系樹脂と同一であることが好ましい。但し、上記中間層に含まれるポリオレフィン系樹脂は、上記基材に含まれるポリオレフィン系樹脂と異なっていてもよい。上記中間層に含まれるポリオレフィン系樹脂は、単独で用いてもよいし、2種以上を併用してもよい。
Polyolefin resin:
The polyolefin resin contained in the intermediate layer is preferably the same as the polyolefin resin contained in the substrate. However, the polyolefin resin contained in the intermediate layer may be different from the polyolefin resin contained in the substrate. The polyolefin resin contained in the intermediate layer may be used alone or in combination of two or more.

上記中間層に含まれるポリオレフィン系樹脂としては、特に限定されないが、エチレン単独重合体、エチレン−α−オレフィン共重合体、エチレン−(メタ)アクリル酸共重合体、エチレン−(メタ)アクリル酸エステル共重合体、及びエチレン−酢酸ビニル共重合体などのポリエチレン系樹脂;プロピレン単独重合体、プロピレン−α−オレフィン共重合体、及びプロピレン−エチレン共重合体などのポリプロピレン系樹脂;ブテン単独重合体;ブタジエン及びイソプレンなどの共役ジエンの単独重合体又は共重合体等が挙げられる。また、上記ポリエチレン系樹脂としては、高密度ポリエチレン及び低密度ポリエチレン等が挙げられる。共重合の形態は、ランダムであってもよく、ブロックであってもよく、三元共重合体の形態であってもよい。   The polyolefin resin contained in the intermediate layer is not particularly limited, but an ethylene homopolymer, an ethylene-α-olefin copolymer, an ethylene- (meth) acrylic acid copolymer, an ethylene- (meth) acrylic acid ester. Polyethylene resins such as copolymers and ethylene-vinyl acetate copolymers; Polypropylene resins such as propylene homopolymers, propylene-α-olefin copolymers, and propylene-ethylene copolymers; Butene homopolymers; Examples include homopolymers or copolymers of conjugated dienes such as butadiene and isoprene. Examples of the polyethylene resin include high density polyethylene and low density polyethylene. The form of copolymerization may be random, block, or terpolymer.

上記ポリエチレン系樹脂は、エチレンを主成分として用いて得られる。上記ポリエチレン系樹脂の全構造単位100重量%中、エチレンに由来する構造単位の割合は好ましくは50重量%以上、より好ましくは70重量%以上、更に好ましくは90重量%以上である。   The polyethylene resin is obtained using ethylene as a main component. The proportion of structural units derived from ethylene is preferably 50% by weight or more, more preferably 70% by weight or more, and still more preferably 90% by weight or more, in 100% by weight of all the structural units of the polyethylene resin.

上記ポリプロピレン系樹脂は、プロピレンを主成分として用いて得られる。上記ポリプロピレン系樹脂の全構造単位100重量%中、プロピレンに由来する構造単位の割合は好ましくは50重量%以上、より好ましくは70重量%以上、更に好ましくは90重量%以上である。   The polypropylene resin is obtained using propylene as a main component. The proportion of structural units derived from propylene is preferably 50% by weight or more, more preferably 70% by weight or more, and still more preferably 90% by weight or more in 100% by weight of all the structural units of the polypropylene resin.

中間層と粘着剤層との層間強度を効果的に高め、表面保護フィルムの取扱い性を効果的に高め、更に表面保護フィルムの高温での寸法安定性をより一層高める観点からは、上記中間層に含まれるポリオレフィン系樹脂は、ポリプロピレン系樹脂であることが好ましい。   From the viewpoint of effectively increasing the interlayer strength between the intermediate layer and the pressure-sensitive adhesive layer, effectively improving the handleability of the surface protective film, and further enhancing the dimensional stability of the surface protective film at high temperatures, the intermediate layer described above is used. The polyolefin-based resin contained in is preferably a polypropylene-based resin.

合成ゴム系粘着剤:
上記中間層に含まれる合成ゴム系粘着剤は、上記粘着剤層に含まれる合成ゴム系粘着剤と同一であることが好ましい。但し、上記中間層に含まれる合成ゴム系粘着剤は、上記粘着剤層に含まれる合成ゴム系粘着剤と異なっていてもよい。上記合成ゴム系粘着剤は、単独で用いてもよいし、2種以上を併用してもよい。
Synthetic rubber adhesive:
The synthetic rubber-based pressure-sensitive adhesive contained in the intermediate layer is preferably the same as the synthetic rubber-based pressure-sensitive adhesive contained in the pressure-sensitive adhesive layer. However, the synthetic rubber pressure sensitive adhesive contained in the intermediate layer may be different from the synthetic rubber pressure sensitive adhesive contained in the pressure sensitive adhesive layer. The said synthetic rubber-type adhesive may be used independently and may use 2 or more types together.

中間層と粘着剤層との層間強度を効果的に高め、表面保護フィルムの取扱い性を効果的に高め、更に表面保護フィルムの高温での寸法安定性をより一層高める観点からは、上記中間層に含まれる合成ゴム系粘着剤は、合成ゴムと粘着付与樹脂とを含むことが好ましい。上記合成ゴムは、単独で用いてもよいし、2種以上を併用してもよい。上記粘着付与樹脂は、単独で用いてもよいし、2種以上を併用してもよい。なお、上記粘着付与樹脂は、使用しなくてもよい。   From the viewpoint of effectively increasing the interlayer strength between the intermediate layer and the pressure-sensitive adhesive layer, effectively improving the handleability of the surface protective film, and further enhancing the dimensional stability of the surface protective film at high temperatures, the intermediate layer described above is used. It is preferable that the synthetic rubber-based pressure-sensitive adhesive contained in contains a synthetic rubber and a tackifying resin. The said synthetic rubber may be used independently and may use 2 or more types together. The above tackifying resins may be used alone or in combination of two or more. The tackifying resin may not be used.

上記中間層に用いることができる合成ゴムとしては、スチレン系エラストマー及びオレフィン系エラストマーなどのエラストマー等が挙げられる。上記エラストマーには、水素添加されたエラストマーが含まれる。   Examples of the synthetic rubber that can be used for the intermediate layer include elastomers such as styrene elastomers and olefin elastomers. The elastomer includes a hydrogenated elastomer.

上記中間層に用いることができるスチレン系エラストマーとしては、ジエンブロック(ジエン重合体部)であるソフトセグメントと、スチレンブロック(スチレン重合体部)であるハードセグメントとを有するブロック共重合体等が挙げられる。上記ジエンブロックは、スチレンとジエンとのランダム構造を有するブロックであってもよい。   Examples of the styrenic elastomer that can be used in the intermediate layer include a block copolymer having a soft segment that is a diene block (diene polymer portion) and a hard segment that is a styrene block (styrene polymer portion). It is done. The diene block may be a block having a random structure of styrene and diene.

上記中間層に用いることができるスチレン系エラストマーの具体例としては、スチレン−ブタジエン(SB)共重合体、スチレン−ブタジエン−スチレン(SBS)共重合体、スチレン−イソプレン(SI)共重合体、スチレン−イソプレン−スチレン(SIS)共重合体、スチレン−エチレン−ブチレン(SEB)共重合体、スチレン−エチレン−ブチレン−スチレン(SEBS)共重合体、スチレン−エチレン−プロピレン(SEP)共重合体、及びスチレン−エチレン−プロピレン−スチレン(SEPS)共重合体などの共重合体が挙げられる。これらの共重合体はブロック共重合体であってもよい。これらの共重合体は、単独で用いてもよいし、2種以上を併用してもよい。   Specific examples of the styrene-based elastomer that can be used for the intermediate layer include styrene-butadiene (SB) copolymer, styrene-butadiene-styrene (SBS) copolymer, styrene-isoprene (SI) copolymer, and styrene. -Isoprene-styrene (SIS) copolymer, styrene-ethylene-butylene (SEB) copolymer, styrene-ethylene-butylene-styrene (SEBS) copolymer, styrene-ethylene-propylene (SEP) copolymer, and Copolymers such as a styrene-ethylene-propylene-styrene (SEPS) copolymer may be mentioned. These copolymers may be block copolymers. These copolymers may be used alone or in combination of two or more.

中間層と粘着剤層との層間強度を効果的に高め、表面保護フィルムの取扱い性を効果的に高め、更に表面保護フィルムの高温での寸法安定性をより一層高める観点からは、上記中間層に含まれる合成ゴム系粘着剤は、好ましくはスチレン系エラストマーであり、より好ましくはSEB共重合体、SEBS共重合体、SEP共重合体、又はSEPS共重合体であり、更に好ましくはSEBS共重合体である。   From the viewpoint of effectively increasing the interlayer strength between the intermediate layer and the pressure-sensitive adhesive layer, effectively improving the handleability of the surface protective film, and further enhancing the dimensional stability of the surface protective film at high temperatures, the intermediate layer described above is used. The synthetic rubber-based pressure-sensitive adhesive contained in is preferably a styrene-based elastomer, more preferably a SEB copolymer, a SEBS copolymer, a SEP copolymer, or a SEPS copolymer, and even more preferably a SEBS copolymer. It is a coalescence.

押出成形時の熱安定性をより一層良好にし、均質な表面保護フィルムを得る観点、並びに中間層と粘着剤層との層間強度を効果的に高め、表面保護フィルムの取扱い性を効果的に高め、更に表面保護フィルムの高温での寸法安定性をより一層高める観点からは、上記中間層に含まれる合成ゴム系粘着剤は、好ましくは水素添加されたスチレン系エラストマーであり、より好ましくは水素添加されたSEB共重合体、水素添加されたSEBS共重合体、水素添加されたSEP共重合体、又は水素添加されたSEPS共重合体であり、更に好ましくは水素添加されたSEBS共重合体である。   From the viewpoint of further improving thermal stability during extrusion, obtaining a homogeneous surface protective film, and effectively increasing the interlayer strength between the intermediate layer and the pressure-sensitive adhesive layer, effectively improving the handleability of the surface protective film Furthermore, from the viewpoint of further enhancing the dimensional stability of the surface protective film at high temperature, the synthetic rubber-based pressure-sensitive adhesive contained in the intermediate layer is preferably a hydrogenated styrene elastomer, more preferably hydrogenated. SEB copolymer, hydrogenated SEBS copolymer, hydrogenated SEP copolymer, or hydrogenated SEPS copolymer, more preferably a hydrogenated SEBS copolymer. .

上記中間層に用いることができるオレフィンエラストマーとしては、結晶性オレフィン−エチレン・ブテン−結晶性オレフィン(CEBC)共重合体、及びスチレン−エチレン・ブテン−結晶性オレフィン(SEBC)共重合体などが挙げられる。これらの共重合体はランダム共重合体であってもブロック共重合体であってもよい。   Examples of the olefin elastomer that can be used in the intermediate layer include a crystalline olefin-ethylene-butene-crystalline olefin (CEBC) copolymer and a styrene-ethylene-butene-crystalline olefin (SEBC) copolymer. It is done. These copolymers may be random copolymers or block copolymers.

上記中間層に用いることができる粘着付与樹脂としては、特に限定されないが、脂肪族系共重合体、芳香族系共重合体、脂肪族・芳香族系共重合体及び脂環式系共重合体等の石油系樹脂、クマロン−インデン系樹脂、テルペン系樹脂、テルペンフェノール系樹脂、重合ロジン等のロジン系樹脂、フェノール系樹脂、キシレン系樹脂等が挙げられる。これらの樹脂は、水素添加された樹脂であってもよい。上記粘着付与樹脂は、単独で用いてもよく、2種以上を併用してもよい。上記粘着付与樹脂が、水素添加された樹脂である場合に剥離性及び耐候性等がより一層高くなる。上記中間層中の粘着付与樹脂は水素添加された樹脂であることが好ましい。   The tackifier resin that can be used in the intermediate layer is not particularly limited, but is an aliphatic copolymer, an aromatic copolymer, an aliphatic / aromatic copolymer, and an alicyclic copolymer. And other petroleum resins, coumarone-indene resins, terpene resins, terpene phenol resins, polymerized rosin and other rosin resins, phenol resins, xylene resins and the like. These resins may be hydrogenated resins. The above tackifying resins may be used alone or in combination of two or more. When the tackifying resin is a hydrogenated resin, the peelability and weather resistance are further enhanced. The tackifying resin in the intermediate layer is preferably a hydrogenated resin.

中間層と基材及び粘着剤層との接着性を高める観点からは、上記中間層中の上記粘着付与樹脂の軟化点は、好ましくは90℃以上、好ましくは140℃以下である。   From the viewpoint of enhancing the adhesion between the intermediate layer and the base material and the pressure-sensitive adhesive layer, the softening point of the tackifying resin in the intermediate layer is preferably 90 ° C. or higher, and preferably 140 ° C. or lower.

上記中間層に含まれる上記合成ゴム系粘着剤において、上記合成ゴム100重量部に対して、上記粘着付与樹脂の含有量は好ましくは5重量部以上、より好ましくは20重量部以上、好ましくは50重量部以下、より好ましくは40重量部以下である。上記粘着付与樹脂の含有量が上記下限以上であると、中間層の基材に対する接着性がより一層高くなり、中間層と粘着剤層との層間強度がより一層高くなる。上記粘着付与樹脂の含有量が上記上限以下であると、中間層の柔軟性がより一層高くなり、表面保護フィルムの取扱い性がより一層高くなり、貼り合わせ品のカールがより一層生じ難くなり、更に表面保護フィルムの高温での寸法安定性がより一層高くなる。   In the synthetic rubber-based pressure-sensitive adhesive contained in the intermediate layer, the content of the tackifying resin is preferably 5 parts by weight or more, more preferably 20 parts by weight or more, preferably 50 parts with respect to 100 parts by weight of the synthetic rubber. It is 40 parts by weight or less, more preferably 40 parts by weight or less. When the content of the tackifying resin is not less than the above lower limit, the adhesion of the intermediate layer to the base material is further increased, and the interlayer strength between the intermediate layer and the pressure-sensitive adhesive layer is further increased. When the content of the tackifying resin is not more than the above upper limit, the flexibility of the intermediate layer is further increased, the handleability of the surface protective film is further increased, and the curling of the bonded product is further less likely to occur. Furthermore, the dimensional stability at a high temperature of the surface protective film is further enhanced.

上記中間層は、回収原料を含む組成物により形成されていることが好ましい。中間層が回収原料により形成される場合に、製造コストを低減することができ、かつ環境負荷を低減することができる。なお、この点については後述する表面保護フィルムの製造方法の欄においても、詳細に説明する。上記回収原料を含む組成物は、回収原料のみを含んでいてもよく、回収原料と新規原料(ポリオレフィン系樹脂、合成ゴム系粘着剤など)とを含んでいてもよい。   It is preferable that the said intermediate | middle layer is formed with the composition containing collection | recovery raw materials. When the intermediate layer is formed from the recovered raw material, the manufacturing cost can be reduced and the environmental load can be reduced. This point will also be described in detail in the column of the method for producing the surface protective film described later. The composition containing the recovered raw material may contain only the recovered raw material, or may contain the recovered raw material and a new raw material (polyolefin resin, synthetic rubber adhesive, etc.).

上記中間層の厚みは、好ましくは10μm以上、より好ましくは20μmを超え、更に好ましくは21μm以上、好ましくは100μm以下、より好ましくは60μm以下である。中間層の厚みが上記下限以上であると、中間層と粘着剤層との層間強度がより一層高くなる。中間層の厚みが上記上限以下であると、表面保護フィルムの外観不良が生じ難くなる。例えば、フィッシュアイと呼ばれる欠点が生じ難くなる。   The thickness of the intermediate layer is preferably 10 μm or more, more preferably more than 20 μm, still more preferably 21 μm or more, preferably 100 μm or less, more preferably 60 μm or less. When the thickness of the intermediate layer is not less than the above lower limit, the interlayer strength between the intermediate layer and the pressure-sensitive adhesive layer is further increased. When the thickness of the intermediate layer is not more than the above upper limit, it becomes difficult to cause a poor appearance of the surface protective film. For example, a defect called fish eye is less likely to occur.

(基材)
上記基材は、ポリオレフィン系樹脂により形成されている。上記基材に含まれる上記ポリオレフィン系樹脂としては、上記中間層に含まれるポリオレフィン系樹脂として例示したポリオレフィン系樹脂等が挙げられる。上記ポリオレフィン系樹脂は、単独で用いてもよいし、2種以上を併用してもよい。
(Base material)
The base material is formed of a polyolefin resin. Examples of the polyolefin resin contained in the substrate include the polyolefin resins exemplified as the polyolefin resin contained in the intermediate layer. The said polyolefin resin may be used independently and may use 2 or more types together.

中間層と粘着剤層との層間強度を効果的に高め、表面保護フィルムの取扱い性を効果的に高め、更に表面保護フィルムの高温での寸法安定性をより一層高める観点からは、上記基材に含まれる上記ポリオレフィン系樹脂は、ポリプロピレン系樹脂であることが好ましい。   From the viewpoint of effectively increasing the interlayer strength between the intermediate layer and the pressure-sensitive adhesive layer, effectively improving the handleability of the surface protective film, and further enhancing the dimensional stability of the surface protective film at high temperatures, The polyolefin resin contained in is preferably a polypropylene resin.

上記基材の厚みは、特に限定されない。上記基材の厚みは好ましくは2μm以上、好ましくは55μm以下である。上記基材の厚みが上記下限以上及び上記上限以下であると、表面保護フィルムの取扱い性が高くなる。   The thickness of the base material is not particularly limited. The thickness of the substrate is preferably 2 μm or more, preferably 55 μm or less. The handleability of a surface protection film becomes it high that the thickness of the said base material is more than the said minimum and below the said upper limit.

(粘着剤層)
上記粘着剤層は、合成ゴム系粘着剤により形成されている。中間層と粘着剤層との層間強度を効果的に高め、表面保護フィルムの取扱い性を効果的に高め、更に表面保護フィルムの高温での寸法安定性をより一層高める観点からは、上記粘着剤層に含まれる上記合成ゴム系粘着剤は、合成ゴムと粘着付与樹脂とを含むことが好ましい。上記合成ゴムは、単独で用いてもよいし、2種以上を併用してもよい。上記粘着付与樹脂は、単独で用いてもよいし、2種以上を併用してもよい。なお、上記粘着付与樹脂は、使用しなくてもよい。
(Adhesive layer)
The pressure-sensitive adhesive layer is formed of a synthetic rubber pressure-sensitive adhesive. From the viewpoint of effectively increasing the interlayer strength between the intermediate layer and the pressure-sensitive adhesive layer, effectively improving the handleability of the surface protective film, and further enhancing the dimensional stability of the surface protective film at high temperatures, the pressure-sensitive adhesive described above. The synthetic rubber-based pressure-sensitive adhesive contained in the layer preferably contains a synthetic rubber and a tackifying resin. The said synthetic rubber may be used independently and may use 2 or more types together. The above tackifying resins may be used alone or in combination of two or more. The tackifying resin may not be used.

上記粘着剤層に用いることができる合成ゴムとしては、スチレン系エラストマー及びオレフィン系エラストマー、アクリル系エラストマー、ウレタン系エラストマー、エステル系エラストマー又はアミド系エラストマーなどのエラストマー等が挙げられる。上記エラストマーには、水素添加されたエラストマーが含まれる。   Examples of the synthetic rubber that can be used for the pressure-sensitive adhesive layer include elastomers such as styrene elastomers and olefin elastomers, acrylic elastomers, urethane elastomers, ester elastomers, and amide elastomers. The elastomer includes a hydrogenated elastomer.

上記粘着剤層に用いることができるスチレン系エラストマーとしては、ジエンブロック(ジエン重合体部)であるソフトセグメントと、スチレンブロック(スチレン重合体部)であるハードセグメントとを有するブロック共重合体等が挙げられる。上記ジエンブロックは、スチレンとジエンとのランダム構造を有するブロックであってもよい。   Examples of the styrenic elastomer that can be used in the pressure-sensitive adhesive layer include a block copolymer having a soft segment that is a diene block (diene polymer portion) and a hard segment that is a styrene block (styrene polymer portion). Can be mentioned. The diene block may be a block having a random structure of styrene and diene.

上記粘着剤層に用いることができるスチレン系エラストマーの具体例としては、上記中間層に用いることができる上記したスチレン系エラストマー等が挙げられる。   Specific examples of the styrene-based elastomer that can be used for the pressure-sensitive adhesive layer include the above-described styrene-based elastomer that can be used for the intermediate layer.

中間層と粘着剤層との層間強度を効果的に高め、表面保護フィルムの取扱い性を効果的に高め、更に表面保護フィルムの高温での寸法安定性をより一層高める観点からは、上記粘着剤層に含まれる合成ゴム系粘着剤は、好ましくはスチレン系エラストマーであり、より好ましくはSEB共重合体、SEBS共重合体、SEP共重合体、又はSEPS共重合体であり、更に好ましくはSEBS共重合体である。   From the viewpoint of effectively increasing the interlayer strength between the intermediate layer and the pressure-sensitive adhesive layer, effectively improving the handleability of the surface protective film, and further enhancing the dimensional stability of the surface protective film at high temperatures, the pressure-sensitive adhesive described above. The synthetic rubber-based pressure-sensitive adhesive contained in the layer is preferably a styrene-based elastomer, more preferably a SEB copolymer, SEBS copolymer, SEP copolymer, or SEPS copolymer, and still more preferably a SEBS copolymer. It is a polymer.

押出成形時の熱安定性をより一層良好にし、均質な表面保護フィルムを得る観点、並びに中間層と粘着剤層との層間強度を効果的に高め、表面保護フィルムの取扱い性を効果的に高め、更に表面保護フィルムの高温での寸法安定性をより一層高める観点からは、上記粘着剤層に含まれる合成ゴム系粘着剤は、好ましくは水素添加されたスチレン系エラストマーであり、より好ましくは水素添加されたSEB共重合体、水素添加されたSEBS共重合体、水素添加されたSEP共重合体、又は水素添加されたSEPS共重合体であり、更に好ましくは水素添加されたSEBS共重合体である。   From the viewpoint of further improving thermal stability during extrusion, obtaining a homogeneous surface protective film, and effectively increasing the interlayer strength between the intermediate layer and the pressure-sensitive adhesive layer, effectively improving the handleability of the surface protective film Further, from the viewpoint of further improving the dimensional stability of the surface protective film at high temperature, the synthetic rubber-based pressure-sensitive adhesive contained in the pressure-sensitive adhesive layer is preferably a hydrogenated styrene-based elastomer, more preferably hydrogen. SEB copolymer added, hydrogenated SEBS copolymer, hydrogenated SEP copolymer, or hydrogenated SEPS copolymer, more preferably hydrogenated SEBS copolymer. is there.

上記粘着剤層に用いることができる上記オレフィン系エラストマーとしては、結晶性オレフィン−エチレン・ブテン−結晶性オレフィン(CEBC)共重合体、及びスチレン−エチレン・ブテン−結晶性オレフィン(SEBC)共重合体などが挙げられる。なお、これらの共重合体は、ランダム共重合体であってもブロック共重合体であってもよい。   Examples of the olefin elastomer that can be used in the pressure-sensitive adhesive layer include a crystalline olefin-ethylene butene-crystalline olefin (CEBC) copolymer, and a styrene-ethylene butene-crystalline olefin (SEBC) copolymer. Etc. In addition, these copolymers may be random copolymers or block copolymers.

上記粘着剤層に用いることができる上記粘着付与樹脂としては、上記中間層に用いることができる上述した粘着付与樹脂等が挙げられる。上記粘着剤層中の粘着付与樹脂は水素添加された樹脂であることが好ましい。   Examples of the tackifier resin that can be used in the pressure-sensitive adhesive layer include the above-described tackifier resins that can be used in the intermediate layer. The tackifier resin in the pressure-sensitive adhesive layer is preferably a hydrogenated resin.

中間層と粘着剤層との接着性を高める観点からは、上記粘着剤層中の上記粘着付与樹脂の軟化点は、好ましくは90℃以上、好ましくは140℃以下である。   From the viewpoint of enhancing the adhesion between the intermediate layer and the pressure-sensitive adhesive layer, the softening point of the tackifying resin in the pressure-sensitive adhesive layer is preferably 90 ° C. or higher, and preferably 140 ° C. or lower.

上記粘着剤層に含まれる上記合成ゴム系粘着剤において、上記合成ゴム100重量部に対して、上記粘着付与樹脂の含有量は好ましくは5重量部以上、より好ましくは20重量部以上、好ましくは50重量部以下、より好ましくは40重量部以下である。上記粘着付与樹脂の含有量が上記下限以上であると、粘着剤層の被着体に対する接着性がより一層高くなり、中間層と粘着剤層との層間強度がより一層高くなる。上記粘着付与樹脂の含有量が上記上限以下であると、粘着剤層の柔軟性がより一層高くなり、表面保護フィルムの取扱い性がより一層高くなり、貼り合わせ品のカールがより一層生じ難くなり、更に表面保護フィルムの高温での寸法安定性がより一層高くなる。   In the synthetic rubber-based pressure-sensitive adhesive contained in the pressure-sensitive adhesive layer, the content of the tackifying resin is preferably 5 parts by weight or more, more preferably 20 parts by weight or more, preferably 100 parts by weight of the synthetic rubber. 50 parts by weight or less, more preferably 40 parts by weight or less. When the content of the tackifying resin is not less than the above lower limit, the adhesiveness of the pressure-sensitive adhesive layer to the adherend is further increased, and the interlayer strength between the intermediate layer and the pressure-sensitive adhesive layer is further increased. When the content of the tackifying resin is not more than the above upper limit, the flexibility of the pressure-sensitive adhesive layer is further enhanced, the handleability of the surface protective film is further enhanced, and the curling of the bonded product is further less likely to occur. Furthermore, the dimensional stability at a high temperature of the surface protective film is further enhanced.

上記粘着剤層の厚みは、特に限定されない。上記粘着剤層の厚みは好ましくは2μm以上、好ましくは15μm以下である。粘着剤層の厚みが上記下限以上であると、より一層均一な厚みの粘着剤層が形成される。粘着剤層の厚みが上記上限以下であると、表面保護フィルムの取扱い性がより一層高くなる。   The thickness of the pressure-sensitive adhesive layer is not particularly limited. The thickness of the pressure-sensitive adhesive layer is preferably 2 μm or more, preferably 15 μm or less. When the thickness of the pressure-sensitive adhesive layer is not less than the above lower limit, a pressure-sensitive adhesive layer having a more uniform thickness is formed. When the thickness of the pressure-sensitive adhesive layer is not more than the above upper limit, the handleability of the surface protective film is further enhanced.

(表面保護フィルムの他の詳細)
表面保護フィルムにおける各層は、特に上記中間層及び上記基材はそれぞれ、本発明の目的を阻害しない範囲で、フェノール系、リン系、アミン系又はイオウ系等の酸化防止剤、ベンゾトリアゾール系又はヒドロキシフェニルトリアジン系等の紫外線吸収剤、金属害防止剤、ヘキサブロモビフェニルエーテル又はデカブロモジフェニルエーテル等のハロゲン化難燃剤、ポリリン酸アンモニウム又はトリメチルフォスフェート等の難燃剤、充填剤、帯電防止剤、安定剤、顔料等の添加剤を含んでいてもよい。これらの添加剤は、単独で用いてもよいし、2種以上を併用してもよい。
(Other details of surface protection film)
Each layer in the surface protective film, in particular, the intermediate layer and the base material are within the range that does not impair the object of the present invention, such as an antioxidant such as phenol, phosphorus, amine, or sulfur, benzotriazole, or hydroxy UV absorbers such as phenyltriazines, metal damage inhibitors, halogenated flame retardants such as hexabromobiphenyl ether or decabromodiphenyl ether, flame retardants such as ammonium polyphosphate or trimethyl phosphate, fillers, antistatic agents, stabilizers In addition, additives such as pigments may be included. These additives may be used independently and may use 2 or more types together.

表面保護フィルムにおける各層は、特に上記中間層及び上記粘着剤層はそれぞれ、本発明の目的を阻害しない範囲で、粘着力の制御等を目的に、必要に応じて、例えば、軟化剤、酸化防止剤及び接着昂進防止剤等の公知の添加剤を含んでいてもよい。これらの添加剤は、単独で用いてもよいし、2種以上を併用してもよい。   Each layer in the surface protective film, in particular, the intermediate layer and the pressure-sensitive adhesive layer are within the range not impairing the object of the present invention, for the purpose of controlling the adhesive force, etc. It may contain known additives such as an agent and an adhesion progress inhibitor. These additives may be used independently and may use 2 or more types together.

上記軟化剤としては、特に限定されないが、低分子量のジエン系ポリマー、ポリイソブチレン水素添加ポリイソプレン、水素添加ポリブタジエン、パラフィン系プロセスオイル、ナフテン系プロセスオイル、芳香族系プロセスオイル、ひまし油、トール油、天然油、液体ポリイソブチレン樹脂、ポリブテン及びこれらの水素添加物などが挙げられる。   The softening agent is not particularly limited, but a low molecular weight diene polymer, polyisobutylene hydrogenated polyisoprene, hydrogenated polybutadiene, paraffinic process oil, naphthenic process oil, aromatic process oil, castor oil, tall oil, Examples thereof include natural oil, liquid polyisobutylene resin, polybutene and hydrogenated products thereof.

上記酸化防止剤としては、例えば、フェノール系酸化防止剤、硫黄系酸化防止剤及びリン系酸化防止剤等が挙げられる。上記フェノール系酸化防止剤としては、モノフェノール系酸化防止剤、ビスフェノール系酸化防止剤及び高分子型フェノール系酸化防止剤等が挙げられる。   As said antioxidant, a phenolic antioxidant, sulfur type antioxidant, phosphorus antioxidant, etc. are mentioned, for example. Examples of the phenolic antioxidant include monophenolic antioxidants, bisphenolic antioxidants, and polymeric phenolic antioxidants.

上記接着昂進防止剤としては、脂肪酸アミド、ポリエチレンイミンの長鎖アルキルグラフト物、大豆油変性アルキド樹脂、トール油及び変性アルキド樹脂等が挙げられる。   Examples of the adhesion progress preventing agent include fatty acid amide, polyethyleneimine long chain alkyl graft product, soybean oil-modified alkyd resin, tall oil, and modified alkyd resin.

上記表面保護フィルムの厚み(基材と中間層と粘着剤層との合計の厚み)は、特に限定されない。上記表面保護フィルムの厚みは好ましくは25μm以上、好ましくは130μm以下である。表面保護フィルムの厚みが上記下限以上であると、表面保護フィルムの取扱い性がより一層高くなり、表面保護フィルムの高温での寸法安定性がより一層高くなる。粘着剤層の厚みが上記上限以下であると、表面保護フィルムの取扱い性がより一層高くなる。   The thickness of the surface protective film (total thickness of the base material, the intermediate layer, and the pressure-sensitive adhesive layer) is not particularly limited. The thickness of the surface protective film is preferably 25 μm or more, and preferably 130 μm or less. When the thickness of the surface protective film is not less than the above lower limit, the handleability of the surface protective film is further enhanced, and the dimensional stability at a high temperature of the surface protective film is further enhanced. When the thickness of the pressure-sensitive adhesive layer is not more than the above upper limit, the handleability of the surface protective film is further enhanced.

(表面保護フィルムの製造方法)
本発明に係る表面保護フィルムは、基材を構成するポリオレフィン系樹脂と、中間層を構成するポリオレフィン系樹脂と合成ゴム系粘着剤とを含む組成物と、粘着剤層を構成する合成ゴム系粘着剤とを、共押出成形により同時に押出して、各層を積層することにより製造できる。表面保護フィルムの製造方法は、共押出成形法に限定されない。表面保護フィルムは、様々な公知の手法により製造可能である。基材上で、中間層及び粘着剤層を形成してもよい。
(Method for producing surface protective film)
The surface protective film according to the present invention comprises a polyolefin resin constituting a base material, a composition comprising a polyolefin resin constituting an intermediate layer and a synthetic rubber adhesive, and a synthetic rubber adhesive constituting an adhesive layer. The agent can be simultaneously extruded by co-extrusion and the layers can be laminated. The method for producing the surface protective film is not limited to the coextrusion molding method. The surface protective film can be produced by various known methods. You may form an intermediate | middle layer and an adhesive layer on a base material.

共押出成形法による製造方法においては、基材上に、中間層、粘着剤層がこの順に積層されるように製造される。上記共押出成形法により製造された表面保護フィルムの端部は、通常、ネックイン現象により厚みが厚くなる。このため、表面保護フィルムの端部、すなわち表面保護フィルムの「耳」は、切断して廃棄されることが多い。   In the manufacturing method by the co-extrusion molding method, the intermediate layer and the pressure-sensitive adhesive layer are manufactured in this order on the base material. The end portion of the surface protective film produced by the coextrusion molding method is usually thick due to a neck-in phenomenon. For this reason, the end portion of the surface protective film, that is, the “ear” of the surface protective film is often cut and discarded.

本発明においては、中間層は、ポリオレフィン基材及び粘着剤層に用いられている原料から構成することが可能である。このため、従来切断して廃棄されていた表面保護フィルムの「耳」等を、回収原料として再利用できる。このように、回収原料を再利用した場合には、製造コストを低減することができ、環境負荷を低減することができる。   In this invention, an intermediate | middle layer can be comprised from the raw material currently used for the polyolefin base material and the adhesive layer. For this reason, the "ear" etc. of the surface protection film conventionally cut and discarded can be reused as a collected raw material. Thus, when the recovered raw material is reused, the manufacturing cost can be reduced and the environmental load can be reduced.

回収原料としては、例えば、表面保護フィルムの作製過程で発生する両端の不要部分(耳)、表面保護フィルムの作製過程で発生する周囲の不要部分、並びに、使用前又は使用済の表面保護フィルムの一部又は全部等が挙げられる。   Examples of the collected raw materials include unnecessary portions (ears) at both ends that are generated in the production process of the surface protective film, unnecessary unnecessary portions that are generated in the production process of the surface protective film, and the surface protective film that is used before or after use. Some or all of them are listed.

回収原料は、基材及び粘着剤層の2層構造を有する表面保護フィルムに由来する原料であってもよく、基材、中間層及び粘着剤層の3層構造を有する表面保護フィルムに由来する原料であってもよい。   The recovered raw material may be a raw material derived from a surface protective film having a two-layer structure of a base material and an adhesive layer, or derived from a surface protective film having a three-layer structure of a base material, an intermediate layer and an adhesive layer. It may be a raw material.

具体的には、例えば、ポリオレフィン系樹脂により形成された基材と合成ゴム系粘着剤により形成された粘着剤層とを備える表面保護フィルムの一部又は全部を、上記中間層の回収原料として用いることができる。さらに、ポリオレフィン系樹脂により形成された基材とポリオレフィン系樹脂及び合成ゴム系粘着剤により形成された中間層と合成ゴム系粘着剤により形成された粘着剤層とを備える表面保護フィルムの一部又は全部も、上記中間層の回収原料として用いることができる。さらに、本発明に係る表面保護フィルムの一部又は全部も、上記中間層の回収原料として用いることができる。   Specifically, for example, a part or all of a surface protective film including a base material formed of a polyolefin-based resin and an adhesive layer formed of a synthetic rubber-based adhesive is used as a recovered material for the intermediate layer. be able to. Furthermore, a part of a surface protection film comprising a base material formed from a polyolefin-based resin, an intermediate layer formed from a polyolefin-based resin and a synthetic rubber-based adhesive, and an adhesive layer formed from a synthetic rubber-based adhesive, or All of them can be used as a raw material for recovering the intermediate layer. Furthermore, part or all of the surface protective film according to the present invention can also be used as the recovered raw material for the intermediate layer.

以下、本発明について、具体的な実施例に基づき、更に詳しく説明する。なお、本発明は以下の実施例に限定されない。   Hereinafter, the present invention will be described in more detail based on specific examples. The present invention is not limited to the following examples.

(実施例1)
各層の材料の準備及び調製:
ポリオレフィン系樹脂(ポリプロピレン、プライムポリマー社製「S135」)を、基材を形成するための材料として用意した。
Example 1
Preparation and preparation of materials for each layer:
A polyolefin resin (polypropylene, “S135” manufactured by Prime Polymer Co., Ltd.) was prepared as a material for forming the base material.

合成ゴム(スチレン−エチレン−ブタジエン−スチレン共重合体であるスチレン系エラストマー、JSR社製「ダイナロン8300P」)100重量部と、粘着付与樹脂(荒川科学社製「アルコンP100」)20重量部とを混合して得られた合成ゴム系粘着剤3重量%と、ポリオレフィン系樹脂(ポリプロピレン、プライムポリマー社製「S135」)97重量%とを混合した混合物を用いて中間層を形成するための組成物を得た。   100 parts by weight of a synthetic rubber (styrene elastomer which is a styrene-ethylene-butadiene-styrene copolymer, “Dynalon 8300P” manufactured by JSR) and 20 parts by weight of a tackifier resin (“Alcon P100” manufactured by Arakawa Scientific) A composition for forming an intermediate layer using a mixture of 3% by weight of a synthetic rubber-based pressure-sensitive adhesive obtained by mixing and 97% by weight of a polyolefin-based resin (polypropylene, “S135” manufactured by Prime Polymer Co., Ltd.) Got.

合成ゴム(スチレン−エチレン−ブタジエン−スチレン共重合体であるスチレン系エラストマー、JSR社製「ダイナロン8300P」)100重量部と、粘着付与樹脂(荒川化学社製「アルコンP100」)20重量部とを混合した混合物を用いて粘着剤層を形成するための合成ゴム粘着剤を得た。   100 parts by weight of a synthetic rubber (styrene elastomer which is a styrene-ethylene-butadiene-styrene copolymer, “DYNARON 8300P” manufactured by JSR) and 20 parts by weight of a tackifier resin (“Alcon P100” manufactured by Arakawa Chemical Co., Ltd.) A synthetic rubber pressure-sensitive adhesive for forming a pressure-sensitive adhesive layer was obtained using the mixed mixture.

表面保護フィルムの作製:
用意した基材層を形成するための材料と、得られた中間層を形成するための組成物と、得られた粘着剤層を形成するための合成ゴム系粘着剤とを、押出機を用いて共押出しすることにより、基材上に中間層及び粘着剤層がこの順に積層された表面保護フィルムを得た。得られた表面保護フィルムにおける各層の厚みに関しては、ポリプロピレン基材の厚みが6μm、中間層の厚みが28μm、粘着剤層の厚みが6μmであった。
Production of surface protective film:
Using an extruder, prepare the material for forming the base material layer, the composition for forming the obtained intermediate layer, and the synthetic rubber-based pressure-sensitive adhesive for forming the obtained pressure-sensitive adhesive layer. The surface protective film in which the intermediate layer and the pressure-sensitive adhesive layer were laminated in this order on the base material was obtained by co-extrusion. Regarding the thickness of each layer in the obtained surface protective film, the thickness of the polypropylene substrate was 6 μm, the thickness of the intermediate layer was 28 μm, and the thickness of the pressure-sensitive adhesive layer was 6 μm.

(実施例2〜8)
中間層に用いるポリオレフィン系樹脂と合成ゴム系粘着剤との配合比を下記の表1に示すように設定したこと、並びに基材、中間層及び粘着剤層の厚みを下記の表1に示すように設定したこと以外は実施例1と同様にして、表面保護フィルムを得た。
(Examples 2 to 8)
As shown in Table 1 below, the compounding ratio of the polyolefin resin used for the intermediate layer and the synthetic rubber adhesive is set as shown in Table 1 below, and the thicknesses of the substrate, the intermediate layer, and the adhesive layer are shown in Table 1 below. A surface protective film was obtained in the same manner as in Example 1 except that it was set to.

参考例9)
粘着付与樹脂を使用せずに中間層及び粘着剤層を作製したこと、中間層に用いるポリオレフィン系樹脂と合成ゴム系粘着剤との配合比を下記の表1に示すように設定したこと、並びに基材、中間層及び粘着剤層の厚みを下記の表1に示すように設定したこと以外は実施例1と同様にして、表面保護フィルムを得た。
( Reference Example 9)
The intermediate layer and the pressure-sensitive adhesive layer were prepared without using a tackifying resin, the compounding ratio of the polyolefin-based resin used for the intermediate layer and the synthetic rubber-based pressure-sensitive adhesive was set as shown in Table 1 below, and A surface protective film was obtained in the same manner as in Example 1 except that the thicknesses of the base material, the intermediate layer and the pressure-sensitive adhesive layer were set as shown in Table 1 below.

(比較例1)
ポリオレフィン系樹脂(ポリプロピレン、プライムポリマー社製「S135」)を、中間層を形成するための材料として用意した。
(Comparative Example 1)
A polyolefin resin (polypropylene, “S135” manufactured by Prime Polymer Co., Ltd.) was prepared as a material for forming the intermediate layer.

中間層を、上記の中間層を形成するための材料を用いて形成したこと以外は実施例1と同様にして、表面保護フィルムを得た。   A surface protective film was obtained in the same manner as in Example 1 except that the intermediate layer was formed using the material for forming the intermediate layer.

(比較例2〜5)
中間層に用いるポリオレフィン系樹脂と合成ゴム系粘着剤との配合比を下記の表1に示すように設定したこと、並びに基材、中間層及び粘着剤層の厚みを下記の表1に示すように設定したこと以外は実施例1と同様にして、表面保護フィルムを得た。
(Comparative Examples 2 to 5)
As shown in Table 1 below, the compounding ratio of the polyolefin resin used for the intermediate layer and the synthetic rubber adhesive is set as shown in Table 1 below, and the thicknesses of the substrate, the intermediate layer, and the adhesive layer are shown in Table 1 below. A surface protective film was obtained in the same manner as in Example 1 except that it was set to.

(評価)
得られた表面保護フィルムについて、以下の評価項目について評価を実施した。
(Evaluation)
About the obtained surface protection film, the following evaluation items were evaluated.

(1)弾性率の低下率
押出し時のMD方向(流れ方向)の寸法が110mm、押出し時のTD方向(MD方向及び厚み方向と直交する方向)の寸法が10mmとなるように、表面保護フィルムを切断し、試験片を得た。テンシロン引張試験機(エーアンドディ社製「STA1255」)を用いて、引張速度300mm/分、23℃及び相対湿度50%RHの条件で、MD方向(流れ方向)に引っ張って、弾性率を測定した。弾性率の低下率は、下記式を用いて算出した。
(1) Decrease rate of elastic modulus Surface protective film so that the dimension in the MD direction (flow direction) during extrusion is 110 mm, and the dimension in the TD direction (direction perpendicular to the MD direction and thickness direction) during extrusion is 10 mm. Was cut to obtain a test piece. Using a Tensilon tensile tester (“STA1255” manufactured by A & D Co., Ltd.), the elastic modulus was measured by pulling in the MD direction (flow direction) under the conditions of a tensile speed of 300 mm / min, 23 ° C. and a relative humidity of 50% RH. did. The decreasing rate of the elastic modulus was calculated using the following formula.

弾性率の低下率(%)=(1−(実施例1〜8、参考例9又は比較例2〜5の各弾性率)/(比較例1の弾性率))×100 Decrease rate of elastic modulus (%) = (1- (each elastic modulus of Examples 1 to 8, Reference Example 9 or Comparative Examples 2 to 5) / (elastic modulus of Comparative Example 1)) × 100

なお、比較例1の表面保護フィルムに関しては、ロール状態の表面保護フィルムを巻き出す際や、表面保護フィルムを被着体に貼り付ける際に、弱い力で引っ張らなくてもよく、作業者が取り扱いやすく、かつは貼り合わせ品にカールが生じなかった。なお、この比較例1の表面保護フィルムでは、中間層と粘接着剤層との層間強度が低い。この比較例1の表面保護フィルムの弾性率を基準として、弾性率が低くなるほど、ロール状態の表面保護フィルムを巻き出す際や、表面保護フィルムを被着体に貼り付ける際に、弱い力で引っ張らなければならず、作業者が取り扱いにくく、かつ貼り合わせ品にカールが生じやすい傾向がある。また、弾性率の低下率を下記の基準で判定した。   The surface protective film of Comparative Example 1 does not have to be pulled with a weak force when unrolling the surface protective film in a roll state or when the surface protective film is attached to the adherend. It was easy and no curling occurred in the bonded product. In the surface protective film of Comparative Example 1, the interlayer strength between the intermediate layer and the adhesive layer is low. With the elastic modulus of the surface protective film of Comparative Example 1 as a reference, the lower the elastic modulus, the lower the surface modulus of the rolled surface protective film, or when the surface protective film is attached to the adherend, it is pulled with a weak force. Therefore, it is difficult for the operator to handle and the bonded product tends to be curled. The rate of decrease in elastic modulus was determined according to the following criteria.

[弾性率の低下率の判定基準]
◎:弾性率の低下率が20%以下
○:弾性率の低下率が20%より大きく、25%以下
×:弾性率の低下率が25%より大きい
[Criteria for rate of decrease in elastic modulus]
A: Decreasing rate of elastic modulus is 20% or less O: Decreasing rate of elastic modulus is greater than 20%, 25% or less X: Decreasing rate of elastic modulus is greater than 25%

(2)加熱収縮率
押出し時のMD方向(流れ方向)の寸法が100mm、押出し時のTD方向(MD方向及び厚み方向と直交する方向)の寸法が100mmとなるように、表面保護フィルムを切断し、試験片を得た。得られた試験片を75℃で30分加熱し、加熱後の寸法からのMD方向及びTD方向における収縮率を、下記式を用いて測定した。また、加熱収縮率を下記の基準で判定した。
(2) Heat shrinkage rate The surface protective film is cut so that the dimension in the MD direction (flow direction) during extrusion is 100 mm, and the dimension in the TD direction (direction perpendicular to the MD direction and the thickness direction) during extrusion is 100 mm. A test piece was obtained. The obtained test piece was heated at 75 ° C. for 30 minutes, and the shrinkage in the MD direction and the TD direction from the dimension after heating was measured using the following formula. Moreover, the heat shrinkage rate was determined according to the following criteria.

加熱収縮率(%)=(加熱前の寸法−加熱後の寸法)×100   Heat shrinkage rate (%) = (dimension before heating−dimension after heating) × 100

[加熱収縮率の判定基準]
○:MD方向及びTD方向の双方の加熱収縮率が±2%の範囲内
×:MD方向及びTD方向のいずれかの加熱収縮率が±2%の範囲を外れる
[Criteria for heat shrinkage]
○: Heat shrinkage in both MD and TD directions is within ± 2% ×: Heat shrinkage in either MD or TD is outside ± 2%

(3)中間層−粘着剤層間の層間強度
押出し時のMD方向(流れ方向)の寸法が100mm、押出し時のTD方向(MD方向及び厚み方向と直交する方向)の寸法が25mmとなるように、表面保護フィルムを切断し、試験片を得た。室温23℃及び相対湿度50%の環境下、2つの試験片を、粘着剤層同士が向かい合うように貼り合わせて、貼り合わせサンプルを得た。貼り合わせサンプルをそれぞれ、室温23℃及び相対湿度50%の環境下、及び室温50℃及び相対湿度50%の環境下で30分放置した。その後、引張速度300mm/分で180°方向に剥離し、剥離した後の剥離面を観察した。中間層−粘着剤層間の層間強度を下記の基準で判定した。
(3) Interlayer strength between the intermediate layer and the adhesive layer The dimension in the MD direction (flow direction) during extrusion is 100 mm, and the dimension in the TD direction (direction perpendicular to the MD direction and thickness direction) during extrusion is 25 mm. The surface protective film was cut to obtain a test piece. In an environment of room temperature 23 ° C. and relative humidity 50%, the two test pieces were bonded so that the pressure-sensitive adhesive layers faced each other, thereby obtaining a bonded sample. The bonded samples were left for 30 minutes at room temperature of 23 ° C. and 50% relative humidity, and at room temperature of 50 ° C. and 50% relative humidity, respectively. Thereafter, the film was peeled in the 180 ° direction at a tensile speed of 300 mm / min, and the peeled surface after peeling was observed. The interlayer strength between the intermediate layer and the adhesive layer was determined according to the following criteria.

[中間層−粘着剤層間の層間強度の判定基準]
○:23℃環境下で放置した貼り合わせサンプル及び50℃環境下で放置した貼り合わせサンプルの双方で、粘着剤層−粘着剤層間で剥離しており、粘着剤層の表面状態に変化が見られない
△:23℃環境下で放置した貼り合わせサンプルで、粘着剤層−粘着剤層間で剥離しており、粘着剤層の表面状態に変化が見られないが、50℃環境下で放置した貼り合わせサンプルで、中間層−粘着剤層間で剥離している
×:23℃環境下で放置した貼り合わせサンプルで、中間層−粘着剤層間で剥離している
[Judgment criteria for interlayer strength between intermediate layer and adhesive layer]
○: In both the bonded sample left under the 23 ° C environment and the bonded sample left under the 50 ° C environment, peeling occurred between the pressure-sensitive adhesive layer and the pressure-sensitive adhesive layer, and a change in the surface state of the pressure-sensitive adhesive layer was observed. △: A pasted sample left in a 23 ° C environment, peeled off between the pressure-sensitive adhesive layer and the pressure-sensitive adhesive layer, and no change was observed in the surface state of the pressure-sensitive adhesive layer, but it was left in a 50 ° C environment. Peeled between the intermediate layer and the pressure-sensitive adhesive layer in the bonded sample. ×: The bonded sample left in an environment at 23 ° C. and peeled between the intermediate layer and the pressure-sensitive adhesive layer.

(4)フィッシュアイの数
表面保護フィルム1mあたりで、0.1mm以上のフィッシュアイがあるか否かを目視で観察した。フィッシュアイの数が少ないほど、欠点が少なく、表面保護フィルムの外観が良好である。フィッシュアイの数を下記の基準で判定した。
(4) Number of fish eyes It was visually observed whether or not there was a fish eye of 0.1 mm or more per 1 m 2 of the surface protective film. The smaller the number of fish eyes, the fewer the defects and the better the appearance of the surface protective film. The number of fish eyes was determined according to the following criteria.

[フィッシュアイの数の判定基準]
○:5個/m未満
△:5個/m以上、10個/m未満
×:10個/m以上
[Criteria for the number of fish eyes]
○: Less than 5 pieces / m 2 Δ: 5 pieces / m 2 or more, less than 10 pieces / m 2 ×: 10 pieces / m 2 or more

詳細及び結果を下記の表1に示す。   Details and results are shown in Table 1 below.

Figure 0006397644
Figure 0006397644

なお、中間層に新規原料を用いて表面保護フィルムを形成した具体的な実施例及び参考例を示した。中間層に新規原料にかえて回収原料を用いて表面保護フィルムを形成した場合でも、本願実施例及び参考例と同様の効果が得られることを確認した。 In addition, the specific Example and reference example which formed the surface protection film using the novel raw material for the intermediate | middle layer were shown. It was confirmed that the same effects as those of the present example and the reference example were obtained even when the surface protective film was formed using the recovered raw material instead of the new raw material in the intermediate layer.

また、実施例1〜3において、中間層−粘着剤層間の層間強度の評価結果はいずれも「○」であるが、実施例3の表面保護フィルムが実施例1,2の表面保護フィルムよりも粘着剤層−粘着剤層間においてより一層スムーズに剥離することができ、実施例2の表面保護フィルムが実施例1の表面保護フィルムよりも粘着剤層−粘着剤層間においてより一層スムーズに剥離することができた。また、実施例6及び参考例9において、中間層−粘着剤層間の層間強度の評価結果はいずれも「△」であるが、実施例6の表面保護フィルムが、参考例9の表面保護フィルムよりも粘着剤層−粘着剤層間においてより一層スムーズに剥離することができた。 Moreover, in Examples 1-3, although the evaluation result of the interlayer strength between an intermediate | middle layer and an adhesive layer is all "(circle)", the surface protection film of Example 3 is more than the surface protection film of Examples 1,2. The surface protective film of Example 2 can be peeled more smoothly between the pressure-sensitive adhesive layer and the pressure-sensitive adhesive layer, and the surface protective film of Example 2 can be peeled more smoothly between the pressure-sensitive adhesive layer and the pressure-sensitive adhesive layer than the surface protective film of Example 1. I was able to. Moreover, in Example 6 and Reference Example 9, the evaluation results of the interlayer strength between the intermediate layer and the adhesive layer are both “Δ”, but the surface protective film of Example 6 is more than the surface protective film of Reference Example 9. Was able to be peeled off more smoothly between the pressure-sensitive adhesive layer and the pressure-sensitive adhesive layer.

Claims (6)

基材と、
前記基材の一方の表面に積層された中間層と、
前記中間層の前記基材側とは反対の表面に積層された粘着剤層とを備え、
前記基材が、ポリプロピレン系樹脂により形成されており、
前記粘着剤層が、合成ゴム系粘着剤により形成されており、
前記中間層が、ポリプロピレン系樹脂85重量%以上、97重量%以下と、合成ゴム系粘着剤3重量%以上、15重量%以下とを含み、
前記中間層に含まれる前記合成ゴム系粘着剤が、合成ゴムと、粘着付与樹脂とを含み、
前記中間層の厚みが、10μm以上、100μm以下である、表面保護フィルム。
A substrate;
An intermediate layer laminated on one surface of the substrate;
A pressure-sensitive adhesive layer laminated on the surface opposite to the base material side of the intermediate layer,
The base material is formed of a polypropylene-based resin;
The pressure-sensitive adhesive layer is formed of a synthetic rubber-based pressure-sensitive adhesive,
The intermediate layer contains polypropylene resin 85% by weight or more and 97% by weight or less, and synthetic rubber adhesive 3% by weight or more and 15% by weight or less,
The synthetic rubber-based pressure-sensitive adhesive contained in the intermediate layer includes a synthetic rubber and a tackifying resin,
The surface protection film whose thickness of the said intermediate | middle layer is 10 micrometers or more and 100 micrometers or less.
前記中間層の厚みが、20μmを超え、60μm以下である、請求項1に記載の表面保護フィルム。   The surface protective film according to claim 1, wherein the intermediate layer has a thickness of more than 20 μm and 60 μm or less. 前記中間層に含まれる前記合成ゴム系粘着剤において、前記合成ゴム100重量部に対する前記粘着付与樹脂の含有量が、5重量部以上、50重量部以下である、請求項1又は2に記載の表面保護フィルム。 In the synthetic rubber adhesive contained in the intermediate layer, the content of the tackifier resin to the synthetic rubber 100 parts by weight, 5 parts by weight or more, 50 parts by weight or less, according to claim 1 or 2 Surface protective film. 前記合成ゴムが、スチレン系エラストマーである、請求項1〜3のいずれか1項に記載の表面保護フィルム。 The synthetic rubber is a styrene-based elastomer, a surface protective film according to any one of claims 1 to 3. 前記スチレン系エラストマーが、水素添加されたスチレン系エラストマーである、請求項に記載の表面保護フィルム。 The surface protective film according to claim 4 , wherein the styrene elastomer is a hydrogenated styrene elastomer. 前記水素添加されたスチレン系エラストマーが、スチレン−エチレン−ブチレン−スチレン共重合体である、請求項に記載の表面保護フィルム。 The surface protective film according to claim 5 , wherein the hydrogenated styrene elastomer is a styrene-ethylene-butylene-styrene copolymer.
JP2014069552A 2014-03-28 2014-03-28 Surface protection film Active JP6397644B2 (en)