JP5380830B2 - Heat-shrinkable polyolefin film and method for producing the same - Google Patents

Heat-shrinkable polyolefin film and method for producing the same Download PDF

Info

Publication number
JP5380830B2
JP5380830B2 JP2007315497A JP2007315497A JP5380830B2 JP 5380830 B2 JP5380830 B2 JP 5380830B2 JP 2007315497 A JP2007315497 A JP 2007315497A JP 2007315497 A JP2007315497 A JP 2007315497A JP 5380830 B2 JP5380830 B2 JP 5380830B2
Authority
JP
Japan
Prior art keywords
film
heat
less
longitudinal direction
shrinkable
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2007315497A
Other languages
Japanese (ja)
Other versions
JP2008174728A (en
Inventor
茂知 山本
幸伸 向山
京子 稲垣
兼次 河井
正敏 橋本
克彦 野瀬
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Toyobo Co Ltd
Original Assignee
Toyobo Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Priority to JP2007315497A priority Critical patent/JP5380830B2/en
Application filed by Toyobo Co Ltd filed Critical Toyobo Co Ltd
Priority to ES07850869T priority patent/ES2380293T3/en
Priority to KR1020097014727A priority patent/KR101380101B1/en
Priority to TW96148554A priority patent/TWI395660B/en
Priority to AT07850869T priority patent/ATE545496T1/en
Priority to PL07850869T priority patent/PL2116354T3/en
Priority to PCT/JP2007/074399 priority patent/WO2008075705A1/en
Priority to EP07850869A priority patent/EP2116354B1/en
Priority to US12/520,193 priority patent/US8697207B2/en
Priority to CN2007800465539A priority patent/CN101583478B/en
Publication of JP2008174728A publication Critical patent/JP2008174728A/en
Application granted granted Critical
Publication of JP5380830B2 publication Critical patent/JP5380830B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は、熱収縮性ポリオレフィン系フィルム、およびその製造方法に関するものであり、詳しくは、ラベル用途に好適な熱収縮性ポリオレフィン系フィルム、およびその製造方法に関するものである。   The present invention relates to a heat-shrinkable polyolefin film and a method for producing the same, and more particularly to a heat-shrinkable polyolefin film suitable for labeling and a method for producing the film.

近年、包装品の外観向上のための外装、内容物の直接的な衝突を避けるための包装、ガラス瓶またはプラスチックボトルの保護と商品の表示を兼ねたラベル包装等の用途に、各種の樹脂からなる熱収縮プラスチックフィルムが広範に使用されている。それらの熱収縮プラスチックフィルムの内、ポリ塩化ビニル系樹脂、ポリスチレン系樹脂、ポリエステル系樹脂、ポリオレフィン系樹脂等からなる延伸フィルムは、ポリエチレンテレフタレート(PET)容器、ポリエチレン容器、ガラス容器等の各種の容器において、ラベルやキャップシールあるいは集積包装の目的で使用される。   In recent years, it has been made of various resins for applications such as exterior packaging for improving the appearance of packages, packaging for avoiding direct collision of contents, and label packaging that also serves to protect glass bottles or plastic bottles and display products. Heat shrink plastic films are widely used. Among these heat-shrinkable plastic films, stretched films made of polyvinyl chloride resin, polystyrene resin, polyester resin, polyolefin resin, etc. are various containers such as polyethylene terephthalate (PET) containers, polyethylene containers, glass containers and the like. In, it is used for the purpose of label, cap seal or integrated packaging.

ところが、ポリ塩化ビニル系フィルムは、収縮特性には優れるものの、耐熱性が低い上に、焼却時に塩化水素ガスを発生したり、ダイオキシンの原因となる等の問題がある。また、ポリ塩化ビニル系樹脂フィルムをPET容器等の収縮ラベルとして用いると、容器をリサイクル利用する際に、ラベルと容器を分離しなければならない、という問題もある。一方、ポリスチレン系フィルムは、収縮後の仕上がり外観性が良好であるものの、耐溶剤性に劣るため、印刷の際に特殊な組成のインキを使用しなければならない、という不具合がある。また、ポリスチレン系フィルムは、高温で焼却する必要がある上に、焼却時に異臭を伴って多量の黒煙が発生するという問題がある。   However, although the polyvinyl chloride film has excellent shrinkage properties, it has low heat resistance and also has problems such as generation of hydrogen chloride gas during incineration and causing dioxins. Further, when a polyvinyl chloride resin film is used as a shrink label for a PET container or the like, there is a problem that the label and the container must be separated when the container is recycled. On the other hand, polystyrene-based films have a good finished appearance after shrinkage, but have poor solvent resistance, so that there is a problem that an ink having a special composition must be used for printing. In addition, the polystyrene film needs to be incinerated at a high temperature and has a problem that a large amount of black smoke is generated with a strange odor during incineration.

それゆえ、耐熱性が高く、焼却が容易であり、耐溶剤性に優れたポリエステル系フィルムやポリオレフィン系フィルムが、収縮ラベルとして広汎に利用されるようになってきており、PET容器の流通量の増大に伴って、使用量が増加している傾向にある。また、通常の熱収縮性ポリエステル系フィルムや熱収縮性ポリオレフィン系フィルムとしては、幅方向に高倍率に延伸されており幅方向に大きく収縮するもの(すなわち、主収縮方向が幅方向であるもの)が広く利用されている(特許文献1)。   Therefore, polyester films and polyolefin films having high heat resistance, easy incineration, and excellent solvent resistance have been widely used as shrink labels, and the amount of PET containers in circulation has been increased. The usage tends to increase with the increase. Moreover, as a normal heat-shrinkable polyester film or heat-shrinkable polyolefin film, a film that is stretched at a high magnification in the width direction and greatly shrinks in the width direction (that is, the main shrinkage direction is the width direction). Is widely used (Patent Document 1).

特開2004−74426号公報JP 2004-74426 A

しかしながら、上記した幅方向に延伸した熱収縮性ポリエステルフィルムや熱収縮性ポリオレフィン系フィルムは、主収縮方向と直交するミシン目に沿って引き裂く場合の引き裂き性(いわゆるミシン目開封性)が悪い、という不具合があった。また、上記した幅方向に延伸した熱収縮性ポリオレフィン系フィルムは、耐熱性が不十分であり、ラベルとして使用した場合に、装着されたボトルを保温器内で保管すると、所謂ブロッキングを起こし、別のボトルのラベルと融着してしまう虞れがある。   However, the heat-shrinkable polyester film and heat-shrinkable polyolefin film stretched in the width direction described above have poor tearability (so-called perforation opening) when tearing along a perforation perpendicular to the main shrinkage direction. There was a bug. In addition, the heat-shrinkable polyolefin film stretched in the width direction described above has insufficient heat resistance, and when used as a label, storing the installed bottle in an incubator causes so-called blocking. There is a risk of fusing with the bottle label.

加えて、幅方向に熱収縮する熱収縮性フィルムは、ボトルのラベルとして装着する際には、幅方向がボトルの周方向となるように筒状体を形成した上で、その筒状体を所定の長さ毎に切断してボトルに装着して熱収縮させなければならないため、高速でボトルに装着するのが困難である。さらに、近年では、お弁当等の合成樹脂製の片開き容器の周囲(開口部)を帯状のフィルムで覆うことによって容器を閉じた状態で保持する新規なラッピング方法が開発されているが、上記した幅方向に収縮するフィルムは、そのような用途に対する使い勝手が悪かった。   In addition, the heat-shrinkable film that heat-shrinks in the width direction is formed as a cylindrical body so that the width direction becomes the circumferential direction of the bottle when the bottle is attached as a bottle label. Since it has to be cut and heat-shrinked into a bottle after every predetermined length, it is difficult to attach it to the bottle at high speed. Furthermore, in recent years, a novel wrapping method has been developed in which a container is closed in a closed state by covering the periphery (opening) of a synthetic resin single-open container such as a lunch box with a belt-like film. The film shrinking in the width direction is not easy to use for such applications.

本発明の目的は、上記従来の熱収縮性ポリエステルフィルムや熱収縮性ポリオレフィン系フィルムが有する問題点を解消し、主収縮方向である長手方向への収縮性が良好である上、ミシン目開封性、耐熱ブロッキング性が良好で、主収縮方向がボトルの周方向になるようにフィルムロールから直接的にボトルの周囲に装着することが可能で、上述した新規なラッピング用途に対する使い勝手の良い実用的な熱収縮性ポリオレフィン系フィルムを提供することにある。   The object of the present invention is to solve the problems of the above-mentioned conventional heat-shrinkable polyester film and heat-shrinkable polyolefin film, and has good shrinkability in the longitudinal direction, which is the main shrinkage direction. Can be installed around the bottle directly from the film roll so that the main shrinkage direction is the circumferential direction of the bottle, and it is practical and easy to use for the above-mentioned new wrapping applications The object is to provide a heat-shrinkable polyolefin film.

本発明のうち、請求項1に記載された発明は、プロピレン−α−オレフィン共重合体を主成分とするポリオレフィン系樹脂によって一定幅の長尺状に形成されており、主収縮方向が長手方向である熱収縮性ポリオレフィン系フィルムであって、脂肪酸アルキルアミン、脂肪酸アルキルアミンエステル、脂肪酸モノグリセリンエステルから選ばれる界面活性剤の帯電防止剤が添加されており、下記要件(1)〜(4)を満たすことを特徴とするものである。
(1)90℃の温水中で10秒間に亘って処理した場合における長手方向の温湯熱収縮率が15%以上40%以下であること
(2)90℃の温水中で10秒間に亘って処理した場合における長手方向と直交する幅方向の温湯熱収縮率が−5%以上10%以下であること
(3)80℃の温水中で長手方向に10%収縮させた後の単位厚み当たりの幅方向の直角引裂強度が50N/mm以上200N/mm以下であること
(4)フィルムの表面同士を合わせて90℃に加熱しながら0.4MPaの圧力を90秒間加えたときの剥離強度が0.1N/15mm以下であること
Among the present inventions, the invention described in claim 1 is formed in a long shape having a constant width by a polyolefin resin mainly composed of a propylene-α-olefin copolymer, and a main shrinkage direction is a longitudinal direction. A heat-shrinkable polyolefin-based film, to which a surfactant antistatic agent selected from fatty acid alkylamines, fatty acid alkylamine esters, and fatty acid monoglycerin esters is added, and the following requirements (1) to (4) It is characterized by satisfying.
(1) The hot water heat shrinkage in the longitudinal direction is 15% or more and 40% or less when treated in 90 ° C. warm water for 10 seconds. (2) Treated in 90 ° C. warm water for 10 seconds. The hot-water heat shrinkage rate in the width direction perpendicular to the longitudinal direction is -5% to 10%. (3) Width per unit thickness after shrinking 10% in the longitudinal direction in hot water at 80 ° C The perpendicular tear strength in the direction is 50 N / mm or more and 200 N / mm or less. (4) The peel strength when a pressure of 0.4 MPa is applied for 90 seconds while the surfaces of the films are combined and heated to 90 ° C. is 0. 1N / 15mm or less

なお、−(マイナス)の温湯熱収縮率は、フィルムの伸長を意味する。   In addition,-(minus) hot-water heat shrinkage rate means the expansion | extension of a film.

請求項2に記載された発明は、請求項1に記載された発明において、ポリオレフィン系樹脂が、プロピレンとエチレンとの共重合体を主成分とするものであり、構成樹脂中のエチレンの量が、2.0質量%以上10.0質量%以下であることを特徴とするものである。   The invention described in claim 2 is the invention described in claim 1, wherein the polyolefin resin is mainly composed of a copolymer of propylene and ethylene, and the amount of ethylene in the constituent resin is 2.0 mass% or more and 10.0 mass% or less.

請求項3に記載された発明は、請求項1に記載された発明において、ポリオレフィン系樹脂が、プロピレンとエチレンとブテンとの共重合体を主成分とするものであり、構成樹脂中のエチレンおよびブテンの量が、3.0質量%以上10.0質量%以下であることを特徴とするものである。   The invention described in claim 3 is the invention described in claim 1, wherein the polyolefin-based resin is mainly composed of a copolymer of propylene, ethylene, and butene. The amount of butene is 3.0% by mass or more and 10.0% by mass or less.

請求項4に記載された発明は、請求項1に記載された発明において、ポリオレフィン系樹脂が、プロピレンとブテンとの共重合体を主成分とするものであり、構成樹脂中のブテンの量が、15.0質量%以上35.0質量%以下であることを特徴とするものである。   The invention described in claim 4 is the invention described in claim 1, wherein the polyolefin resin is mainly composed of a copolymer of propylene and butene, and the amount of butene in the constituent resin is 15.0 mass% or more and 35.0 mass% or less.

請求項5に記載された発明は、請求項1〜4のいずれかに記載された発明において、コア層の少なくとも片面にスキン層を積層した積層構造を有しており、前記スキン層中に、アンチブロッキング剤および/または脂肪酸アルキルアミン、脂肪酸アルキルアミンエステル、脂肪酸モノグリセリンエステルから選ばれる界面活性剤の帯電防止剤が添加されていることを特徴とするものである。 The invention described in claim 5 has the laminated structure in which the skin layer is laminated on at least one surface of the core layer in the invention described in any one of claims 1 to 4, and the skin layer includes: An anti-blocking agent and / or a surfactant antistatic agent selected from fatty acid alkylamines, fatty acid alkylamine esters, and fatty acid monoglycerin esters are added.

請求項6に記載された発明は、請求項1〜5のいずれかに記載の熱収縮性ポリオレフィン系フィルムを製造するための製造方法であって、未延伸フィルムを、テンター内で幅方向の両端際をクリップによって把持した状態で70℃以上140℃以下の温度で幅方向に2.5倍以上8.0倍以下の倍率で延伸した後に、100℃以上155℃以下の温度で1.0秒以上50.0秒以下の時間に亘って熱処理し、しかる後、フィルムの幅方向の両端縁のクリップ把持部分を切断除去した後、70℃以上140℃以下の温度で長手方向に2.0倍以上8.0倍以下の倍率で延伸することを特徴とするものである。   Invention of Claim 6 is a manufacturing method for manufacturing the heat-shrinkable polyolefin-type film in any one of Claims 1-5, Comprising: An unstretched film is made into the both ends of the width direction within a tenter. After being stretched by a clip at a temperature of 70 ° C. or higher and 140 ° C. or lower at a magnification of 2.5 times or more and 8.0 times or less, the film is stretched at a temperature of 100 ° C. or higher and 155 ° C. or lower for 1.0 second. After heat treatment for a time of 50.0 seconds or less and then cutting and removing the clip gripping portions at both edges in the width direction of the film, the film is 2.0 times longer in the longitudinal direction at a temperature of 70 ° C. or more and 140 ° C. or less. The film is drawn at a magnification of 8.0 times or less.

本発明の熱収縮性ポリオレフィン系フィルムは、主収縮方向である長手方向への収縮性が高い上、主収縮方向と直交する方向のミシン目開封性が良好である。したがって、ボトル等の容器のラベルとして好適に用いることができ、短時間の内に非常に効率良く容器に装着することができ、装着して熱収縮させた際に、熱収縮によるシワや収縮不足のきわめて少ない良好な仕上がりを呈するとともに、非常に良好なミシン目開封性を発現する。さらに、ボトル等の容器のラベルとして使用した際に、耐熱ブロッキング性が良好である。加えて、上述した新規なラッピング用途に対する使い勝手も良好である。   The heat-shrinkable polyolefin film of the present invention has high shrinkability in the longitudinal direction, which is the main shrinkage direction, and also has good perforation openability in the direction perpendicular to the main shrinkage direction. Therefore, it can be suitably used as a label for containers such as bottles, and can be attached to containers very efficiently within a short period of time. In addition to exhibiting a very good finish with a very low perforation, it exhibits a very good perforation opening. Furthermore, when used as a label for a container such as a bottle, the heat blocking property is good. In addition, the usability for the above-described novel lapping application is also good.

また、本発明の熱収縮性ポリオレフィン系フィルムの製造方法によれば、上記の如く長手方向への収縮性が高く、収縮仕上がり性、ミシン目開封性、耐熱ブロッキング性が良好な熱収縮性ポリオレフィン系フィルムを、安価かつ容易に製造することができる。   In addition, according to the method for producing a heat-shrinkable polyolefin film of the present invention, the heat-shrinkable polyolefin film has high shrinkability in the longitudinal direction as described above, and has good shrinkage finish, perforation opening property, and heat-resistant blocking property. The film can be manufactured inexpensively and easily.

本発明で用いるプロピレンと他のα−オレフィンとの共重合体のα−オレフィン共重合成分としては、炭素数が2〜8のα−オレフィン、たとえば、エチレン、ブテン−1等が好ましく、ペンテン−1、ヘキセン−1、4−メチル−1−ペンテン等を用いることも可能である。また、共重合体は、プロピレンに上記に例示されるα−オレフィンを1種または2種以上重合して得られたランダムまたはブロック共重合体であることが好ましい。さらに、それらの共重合体の中でも、プロピレンとエチレンとを共重合させたものであってエチレンの量が2.0質量%以上10.0質量%以下であるもの、プロピレンとブテンとを共重合させたものであってブテンの量が15.0質量%以上35.0質量%以下であるもの、プロピレンとエチレンとブテンとを共重合させたものであってエチレンおよびブテンの量が3.0質量%以上15.0質量%以下であるものを使用すると、良好な収縮特性が得られるので特に好ましい。   The α-olefin copolymerization component of the copolymer of propylene and other α-olefin used in the present invention is preferably an α-olefin having 2 to 8 carbon atoms, such as ethylene, butene-1, and the like. 1, hexene-1,4-methyl-1-pentene and the like can also be used. The copolymer is preferably a random or block copolymer obtained by polymerizing one or more of the α-olefins exemplified above with propylene. Further, among these copolymers, propylene and ethylene are copolymerized and the amount of ethylene is 2.0% by mass or more and 10.0% by mass or less, and propylene and butene are copolymerized. In which the amount of butene is 15.0% by mass or more and 35.0% by mass or less, copolymerized propylene, ethylene and butene, and the amount of ethylene and butene is 3.0. It is particularly preferable to use a material having a mass percentage of 15.0 mass% because good shrinkage characteristics can be obtained.

また、共重合体のメルトフローレート(MFR)は、0.1〜100g/10min.の範囲内であると好ましく、0.5〜20g/10min.の範囲内であるとより好ましく、1.0〜10g/10min.の範囲内であると特に好ましい。また、本発明に用いる樹脂の融点は、70℃以上150℃以下であると好ましく、80℃以上145℃以下であるとより好ましく、90℃以上140℃以下であると特に好ましい。融点が150℃を超えると、結晶性が高くなり、十分な収縮特性が得られないため、好ましくなく、反対に70℃を下回ると、樹脂にベタツキ、ブロッキングが発生し、取り扱いが困難となる場合があり、好ましくない。   Further, the melt flow rate (MFR) of the copolymer is 0.1 to 100 g / 10 min. Is preferably in the range of 0.5 to 20 g / 10 min. More preferably, it is in the range of 1.0 to 10 g / 10 min. It is especially preferable that it is within the range. The melting point of the resin used in the present invention is preferably 70 ° C. or higher and 150 ° C. or lower, more preferably 80 ° C. or higher and 145 ° C. or lower, and particularly preferably 90 ° C. or higher and 140 ° C. or lower. If the melting point exceeds 150 ° C, the crystallinity becomes high and sufficient shrinkage characteristics cannot be obtained. This is not preferable. On the other hand, if the melting point is below 70 ° C, the resin becomes sticky or blocked, making handling difficult. Is not preferable.

本発明において、用いる樹脂には必要に応じて、特性を阻害しない範囲で、各種添加材、充填材、たとえば、熱安定剤、酸化防止剤、光安定剤、帯電防止剤、滑剤、核剤、難燃剤、顔料、染料、炭酸カルシウム、硫酸バリウム、水酸化マグネシウム、マイカ、タルク、クレー、酸化亜鉛、酸化マグネシウム、酸化アルミニウム、抗菌剤、防曇剤、自然分解性を付与する添加剤等を添加することができる。特に、取り扱い性の面、および、滑り性、帯電防止性、耐熱ブロッキング性を付与する意味から、脂肪酸アミドに代表される有機系滑剤や脂肪酸アルキルアミン、脂肪酸アルキルアミンエステル、脂肪酸モノグリセリンエステルに代表される界面活性剤、シリカ、PMMAに代表されるアンチブロッキング剤を添加することが好ましい。さらにまた、その他の熱可塑性樹脂、熱可塑性エラストマー、ゴム類、炭化水素樹脂、石油樹脂等を本発明のフイルムの特性を害さない範囲で配合しても良い。   In the present invention, if necessary, the resin used may be various additives and fillers, for example, a heat stabilizer, an antioxidant, a light stabilizer, an antistatic agent, a lubricant, a nucleating agent, as long as the properties are not impaired. Adds flame retardants, pigments, dyes, calcium carbonate, barium sulfate, magnesium hydroxide, mica, talc, clay, zinc oxide, magnesium oxide, aluminum oxide, antibacterial agents, antifogging agents, additives that impart natural degradability, etc. can do. In particular, organic lubricants such as fatty acid amides, fatty acid alkylamines, fatty acid alkylamine esters, and fatty acid monoglycerin esters are representative of handling properties and the meaning of imparting slipperiness, antistatic properties, and heat blocking properties. It is preferable to add an antiblocking agent typified by a surfactant, silica, and PMMA. Furthermore, other thermoplastic resins, thermoplastic elastomers, rubbers, hydrocarbon resins, petroleum resins, and the like may be blended within a range that does not impair the characteristics of the film of the present invention.

さらに、本発明のフイルムは、その特性を阻害しない範囲で、表面に同種のポリプロピレン系樹脂層および他の樹脂層、たとえば、エチレン−酢酸ビニル共重合体けん化物、ポリビニルアルコール等のガスバリア性樹脂層を積層しても良い。   Furthermore, the film of the present invention has the same type of polypropylene resin layer and other resin layers on the surface thereof, for example, a saponified ethylene-vinyl acetate copolymer, a gas barrier resin layer such as polyvinyl alcohol, etc., as long as the properties are not impaired. May be laminated.

本発明のフイルムには、必要に応じて本発明の特性を阻害しない範囲で、表面処理を行うことができる。表面処理の方法としては、コロナ放電処理、プラズマ処理、火炎処理、酸処理等を例示することができ、特に制限はない。連続処理が可能であり、このフイルムの製造過程の巻き取り工程前に容易に実施できるコロナ放電処理、プラズマ処理、火炎処理を行うのが好ましく、熱融着層表面の濡れ張力を向上させる手段としてはコロナ放電処理が特に好ましい。   The film of the present invention can be subjected to surface treatment within a range that does not impair the characteristics of the present invention, if necessary. Examples of the surface treatment method include corona discharge treatment, plasma treatment, flame treatment, and acid treatment, and are not particularly limited. It is preferable to perform corona discharge treatment, plasma treatment, and flame treatment that can be carried out continuously and can be easily performed before the winding process of the film production process. Is particularly preferably a corona discharge treatment.

また、本発明の熱収縮性ポリオレフィン系フィルムは、90℃の温水中で無荷重状態で10秒間に亘って処理したときに、収縮前後の長さから、下式1により算出したフィルムの長手方向の熱収縮率(すなわち、90℃の温湯熱収縮率)が、15%以上40%以下であることが必要である。
熱収縮率={(収縮前の長さ−収縮後の長さ)/収縮前の長さ}×100(%) ・・式1
In addition, the heat-shrinkable polyolefin film of the present invention is the longitudinal direction of the film calculated by the following formula 1 from the length before and after shrinkage when treated for 10 seconds in 90 ° C. warm water without load. The heat shrinkage ratio (that is, hot water heat shrinkage ratio at 90 ° C.) of 15% or more and 40% or less is required.
Thermal shrinkage rate = {(length before shrinkage−length after shrinkage) / length before shrinkage} × 100 (%)

90℃における長手方向の温湯熱収縮率が15%未満であると、収縮量が小さいために、熱収縮した後のラベルにシワやタルミが生じてしまうので好ましくない。なお、90℃における長手方向の温湯熱収縮率の下限値は、18%以上であると好ましく、21%以上であるとより好ましく、24%以上であると特に好ましい。なお、原料であるプロピレン−α−オレフィン共重合体を主成分とするポリオレフィン系樹脂の本質的な特性を考慮すると、90℃における長手方向の温湯熱収縮率の上限値は、40%程度と考えている。   When the hot-water heat shrinkage rate in the longitudinal direction at 90 ° C. is less than 15%, the shrinkage amount is small, and thus wrinkles and tarmi are generated on the label after heat shrinkage, which is not preferable. In addition, the lower limit of the hot water heat shrinkage in the longitudinal direction at 90 ° C. is preferably 18% or more, more preferably 21% or more, and particularly preferably 24% or more. In addition, considering the essential characteristics of the polyolefin-based resin mainly composed of the raw material propylene-α-olefin copolymer, the upper limit value of the hot water heat shrinkage in the longitudinal direction at 90 ° C. is considered to be about 40%. ing.

また、本発明の熱収縮性ポリオレフィン系フィルムは、90℃の温水中で無荷重状態で10秒間に亘って処理したときに、収縮前後の長さから、上式1により算出したフィルムの幅方向の温湯熱収縮率が、−5%以上10%以下であることが必要である。   The heat-shrinkable polyolefin film of the present invention is a film width direction calculated by the above formula 1 from the length before and after shrinkage when treated for 10 seconds in 90 ° C. warm water under no load. It is necessary that the hot-water heat shrinkage rate is -5% or more and 10% or less.

90℃における幅方向の温湯熱収縮率が10%を上回ると、ラベルとして用いた場合に熱収縮時に縦ひけが生じ易くなるので好ましくない。なお、90℃における幅方向の温湯熱収縮率の下限値は、−3%以上であると好ましく、−1%以上であるとより好ましい。また、90℃における幅方向の温湯熱収縮率の上限値は、9%以下であると好ましく、8%以下であるとより好ましく、7%以下であると特に好ましい。また、原料であるプロピレン−α−オレフィン共重合体を主成分とするポリオレフィン系樹脂の本質的な特性を考慮すると、90℃における幅方向の温湯熱収縮率の下限値は、−5%程度と考えている。   If the hot-water heat shrinkage in the width direction at 90 ° C. exceeds 10%, it is not preferable because vertical sink marks are likely to occur during heat shrinkage when used as a label. In addition, the lower limit of the hot water heat shrinkage in the width direction at 90 ° C. is preferably −3% or more, and more preferably −1% or more. Moreover, the upper limit of the hot water heat shrinkage in the width direction at 90 ° C. is preferably 9% or less, more preferably 8% or less, and particularly preferably 7% or less. In addition, considering the essential characteristics of the polyolefin-based resin whose main component is a propylene-α-olefin copolymer, the lower limit value of the hot water heat shrinkage in the width direction at 90 ° C. is about −5%. thinking.

また、本発明の熱収縮性ポリオレフィン系フィルムは、80℃の温水中で長手方向に10%収縮させた後に、以下の方法で単位厚み当たりの幅方向の直角引裂強度を求めたときに、その幅方向の直角引裂強度が50N/mm以上200N/mm以下であることが必要である。   Further, the heat-shrinkable polyolefin film of the present invention was subjected to 10% shrinkage in the longitudinal direction in warm water at 80 ° C., and then the right-angled tear strength per unit thickness was determined by the following method. The right-angled tear strength in the width direction is required to be 50 N / mm or more and 200 N / mm or less.

[直角引裂強度の測定方法]
80℃に調整された温湯中にてフィルムを長手方向に10%収縮させた後に、JIS−K−7128に準じて所定の大きさの試験片としてサンプリングする。しかる後に、万能引張試験機で試験片の両端を掴み、引張速度200mm/分の条件にて、フィルムの幅方向における引張破壊時の強度の測定を行う。なお、80℃で10%収縮しないフィルムについては、約5秒間に亘って80℃の温水に浸漬させることによって収縮可能な分だけ収縮させたフィルムの幅方向における引張破壊時の強度の測定を行う。そして、下式2を用いて単位厚み当たりの直角引裂強度を算出する。
直角引裂強度=引張破壊時の強度÷厚み ・・式2
[Measurement method of right-angle tear strength]
The film is contracted 10% in the longitudinal direction in hot water adjusted to 80 ° C., and then sampled as a test piece of a predetermined size according to JIS-K-7128. Thereafter, both ends of the test piece are grasped with a universal tensile tester, and the strength at the time of tensile fracture in the width direction of the film is measured under the condition of a tensile speed of 200 mm / min. In addition, about the film which does not shrink 10% at 80 degreeC, the intensity | strength at the time of the tensile fracture in the width direction of the film shrunk by the part which can be shrunk by immersing in warm water of 80 degreeC over about 5 second is measured. . Then, the right angle tear strength per unit thickness is calculated using the following equation 2.
Right angle tear strength = Strength at tensile fracture ÷ thickness ・ ・ Equation 2

80℃の温水中で長手方向に10%収縮させた後の直角引裂強度が50N/mm未満であると、ラベルとして使用した場合に運搬中の落下等の衝撃によって簡単に破れてしまう事態が生ずる可能性があるので好ましくなく、反対に、直角引裂強度が200N/mmを上回ると、ラベルを引き裂く際の初期段階におけるカット性(引き裂き易さ)が不良となるため好ましくない。なお、直角引裂強度の下限値は、70N/mm以上であると好ましく、90N/mm以上であるとより好ましく、110N/mm以上であると特に好ましい。また、直角引裂強度の上限値は、180N/mm以下であると好ましく、160N/mm以下であるとより好ましく、140N/mm以下であると特に好ましい。   When the right-angled tear strength after shrinking 10% in the longitudinal direction in warm water at 80 ° C is less than 50 N / mm, when used as a label, it may be easily broken by impact such as dropping during transportation. On the contrary, if the right-angled tear strength exceeds 200 N / mm, the cutting property (easy to tear) at the initial stage of tearing the label becomes unfavorable. The lower limit of the right-angled tear strength is preferably 70 N / mm or more, more preferably 90 N / mm or more, and particularly preferably 110 N / mm or more. Moreover, the upper limit value of the right-angled tear strength is preferably 180 N / mm or less, more preferably 160 N / mm or less, and particularly preferably 140 N / mm or less.

なお、ラベルをミシン目部分において引裂く際のカット性に関しては、上記に記載したようなミシン目の最初の部分(ラベルの上端あるいは下端の部分)の引裂き易さ(切り欠きの入り易さ)と、ミシン目に沿って斜めにずれたり途中でタブが切れたりせず、軽い力でミシン目方向に最後まで裂けるような引裂き易さ(ミシン目方向と直角方向との引裂き易さのバランス)との両方が、実際に手でラベルを剥がす際の作業のし易さに寄与するものと考えるが、後者はミシン目のピッチの改良等により幾分改善することができるようになり、また前者のミシン目の最初の部分の引裂き易さの方が、実際に手でラベルを引裂く際の官能評価とよりよく対応しており、より重要な特性と考えられる。従って、本発明の熱収縮ポリオレフィン系フィルムは上記範囲の直角引裂強度であることが必要である。しかし、後者のミシン目方向と直角方向との引裂き易さのバランスをある特定の範囲にすることは本発明の熱収縮ポリオレフィン系フィルムのミシン目開封性をより向上させることができるので好ましい。具体的には、本発明の熱収縮性ポリオレフィン系フィルムは、80℃の温水中で長手方向に10%収縮させた後に、以下の方法で長手方向および幅方向のエルメンドルフ引裂荷重を求めたときに、それらのエルメンドルフ引裂荷重の比であるエルメンドルフ比が0.15以上1.5以下であることが好ましい。   Regarding the cutability when tearing the label at the perforated part, the ease of tearing (the ease of notching) of the first part of the perforated line (the upper or lower part of the label) as described above And easy to tear along the perforation without breaking diagonally or cutting the tab in the middle and tearing in the direction of the perforation to the end with a light force (balance of ease of tearing between the perforation direction and the perpendicular direction) Both of them contribute to the ease of work when actually peeling the label by hand, but the latter can be improved somewhat by improving the pitch of the perforation, etc. The ease of tearing of the first part of the perforation corresponds to the sensory evaluation when actually tearing the label by hand, and is considered to be a more important characteristic. Therefore, the heat-shrinkable polyolefin film of the present invention needs to have a right angle tear strength in the above range. However, it is preferable to set the balance of the ease of tearing in the latter perforation direction and the perpendicular direction within a certain range because the perforation opening property of the heat-shrinkable polyolefin film of the present invention can be further improved. Specifically, when the heat-shrinkable polyolefin film of the present invention was subjected to 10% shrinkage in the longitudinal direction in warm water at 80 ° C., the Elmendorf tear load in the longitudinal direction and the width direction was determined by the following method. The Elmendorf ratio, which is the ratio of these Elmendorf tear loads, is preferably 0.15 or more and 1.5 or less.

[エルメンドルフ比の測定方法]
所定の長さを有する矩形状の枠にフィルムを予め弛ませた状態で装着する(すなわち、フィルムの両端を枠によって把持させる)。そして、弛んだフィルムが枠内で緊張状態となるまで(弛みがなくなるまで)、約5秒間に亘って80℃の温水に浸漬させることによって、フィルムを長手方向に10%収縮させる。しかる後に、JIS−K−7128に準じて、フィルムの長手方向および幅方向のエルメンドルフ引裂荷重の測定を行い、下式3を用いてエルメンドルフ比を算出する。なお、80℃で10%収縮しないフィルムについては、約5秒間に亘って80℃の温水に浸漬させることによって収縮可能な分だけ収縮させたフィルムの長手方向および幅方向のエルメンドルフ引裂荷重の測定を行う。
エルメンドルフ比=長手方向のエルメンドルフ引裂荷重÷幅方向のエルメンドルフ引裂荷重 ・・式3
[Measurement method of Elmendorf ratio]
The film is attached to a rectangular frame having a predetermined length in a state of being loosened in advance (that is, both ends of the film are gripped by the frame). Then, the film is contracted by 10% in the longitudinal direction by immersing in warm water at 80 ° C. for about 5 seconds until the slack film is in a tension state in the frame (until the slack disappears). Thereafter, the Elmendorf tear load in the longitudinal direction and the width direction of the film is measured according to JIS-K-7128, and the Elmendorf ratio is calculated using the following equation 3. For films that do not shrink 10% at 80 ° C., measure the Elmendorf tear load in the longitudinal and width directions of the film that has been shrunk as much as possible by being immersed in warm water at 80 ° C. for about 5 seconds. Do.
Elmendorf ratio = Elmendorf tear load in the longitudinal direction ÷ Elmendorf tear load in the width direction.

エルメンドルフ比が0.15未満であると、ラベルとして使用した場合にミシン目に沿って真っ直ぐに引き裂きにくいので好ましくない。反対にエルメンドルフ比が1.5を上回ると、ミシン目とずれた位置で裂け易くなるので好ましくない。なお、エルメンドルフ比の下限値は、0.20以上であると好ましく、0.25以上であるとより好ましく、0.3以上であると特に好ましい。また、エルメンドルフ比の上限値は、1.4以下であると好ましく、1.3以下であるとより好ましく、1.2以下であると特に好ましい。   If the Elmendorf ratio is less than 0.15, it is not preferable because it is difficult to tear straight along the perforation when used as a label. On the other hand, if the Elmendorf ratio exceeds 1.5, it is not preferable because it is easy to tear at a position shifted from the perforation. The lower limit value of the Elmendorf ratio is preferably 0.20 or more, more preferably 0.25 or more, and particularly preferably 0.3 or more. The upper limit value of the Elmendorf ratio is preferably 1.4 or less, more preferably 1.3 or less, and particularly preferably 1.2 or less.

さらに、本発明の熱収縮性ポリオレフィン系フィルムは、フィルムの表面同士を合わせて90℃に加熱しながら0.4MPaの圧力を90秒間加えたときの剥離強度(以下、耐熱剥離強度という)が0.1N/15mm以下であることが必要である。かかる耐熱剥離強度は、万能引張試験機で重なった2枚の各フィルムの両端を掴み、引張速度200mm/分の条件にて、2枚のフィルムを剥離させた際の強度を測定することによって求めることができる。耐熱剥離強度が、0.1N/mmを上回ると、熱収縮性ポリオレフィン系フィルムをラベルとした際に、加熱により(たとえば、ラベルを被覆したPETボトルを保温器で保存することにより)ブロッキングを起こす虞れがあるので好ましくない。なお、耐熱剥離強度は、0.05N/mm以下であると好ましく、0N/mmであると最も好ましい。   Furthermore, the heat-shrinkable polyolefin film of the present invention has a peel strength (hereinafter referred to as heat-resistant peel strength) of 0 when a pressure of 0.4 MPa is applied for 90 seconds while the surfaces of the films are combined and heated to 90 ° C. .1 N / 15 mm or less is required. Such heat-resistant peel strength is obtained by grasping both ends of each of the two overlapped films with a universal tensile tester and measuring the strength when the two films are peeled off under a tensile speed of 200 mm / min. be able to. When the heat-resistant peel strength exceeds 0.1 N / mm, when a heat-shrinkable polyolefin film is used as a label, blocking is caused by heating (for example, by storing a PET bottle coated with the label in an incubator). Since there is a fear, it is not preferable. The heat-resistant peel strength is preferably 0.05 N / mm or less, and most preferably 0 N / mm.

上記の熱収縮フィルムの熱収縮率、直角引裂強度、エルメンドルフ比、耐熱剥離強度は、前述の好ましいフィルム組成を用いて、後述の好ましい製造方法と組み合わせることにより達成することが可能となる。   The heat shrinkage rate, right-angle tear strength, Elmendorf ratio, and heat-resistant peel strength of the heat shrinkable film can be achieved by using the preferred film composition described above and combining with the preferred production method described later.

本発明の熱収縮性ポリオレフィン系フィルムの厚みは、特に限定するものではないが、ラベル用熱収縮性フィルムとして10〜200μmが好ましく、20〜100μmがより好ましい。   Although the thickness of the heat-shrinkable polyolefin film of the present invention is not particularly limited, the heat-shrinkable film for labels is preferably 10 to 200 μm, and more preferably 20 to 100 μm.

また、本発明の熱収縮性ポリオレフィン系フィルムは、上記したポリオレフィン系樹脂原料を押出機により溶融押し出しして未延伸フィルムを形成し、その未延伸フィルムを以下に示す方法により、二軸延伸して熱処理することによって得ることができる。   Further, the heat-shrinkable polyolefin film of the present invention is obtained by melting and extruding the above-mentioned polyolefin resin raw material with an extruder to form an unstretched film, and biaxially stretching the unstretched film by the method shown below. It can be obtained by heat treatment.

原料樹脂を溶融押し出しする際には、ポリオレフィン系樹脂原料をホッパードライヤー、パドルドライヤー等の乾燥機、または真空乾燥機を用いて乾燥するのが好ましい。そのようにポリオレフィン系樹脂原料を乾燥させた後に、押出機を利用して、200〜300℃の温度で溶融しフィルム状に押し出す。かかる押し出しに際しては、Tダイ法、チューブラー法等、既存の任意の方法を採用することができる。   When the raw material resin is melt-extruded, the polyolefin resin raw material is preferably dried using a dryer such as a hopper dryer or a paddle dryer, or a vacuum dryer. After the polyolefin-based resin raw material is dried in such a manner, it is melted at a temperature of 200 to 300 ° C. and extruded into a film using an extruder. For this extrusion, any existing method such as a T-die method or a tubular method can be employed.

そして、押し出し後のシート状の溶融樹脂を急冷することによって未延伸フィルムを得ることができる。なお、溶融樹脂を急冷する方法としては、溶融樹脂を口金より回転ドラム上にキャストして急冷固化することにより実質的に未配向の樹脂シートを得る方法を好適に採用することができる。   And an unstretched film can be obtained by rapidly cooling the sheet-like molten resin after extrusion. In addition, as a method of rapidly cooling the molten resin, a method of obtaining a substantially unoriented resin sheet by casting the molten resin on a rotating drum from a die and rapidly solidifying it can be suitably employed.

さらに、得られた未延伸フィルムを、後述するように、所定の条件で幅方向に延伸した後に、一旦、熱処理し、しかる後に所定の条件で長手方向に延伸し、その縦延伸後のフィルムを急冷することによって、本発明の熱収縮性ポリオレフィン系フィルムを得ることが可能となる。なお、縦延伸する際には、延伸ギャップ(縦延伸する際の低速ロールとフィルムとの接点から高速ロールとフィルムとの接点までの距離)とフィルム幅とを適宜調整することによって、ギャップ比率(延伸ギャップ/フィルム幅)を0.01〜0.10の範囲に調整することができる。   Further, as will be described later, the obtained unstretched film was stretched in the width direction under predetermined conditions, and then heat-treated once, and then stretched in the longitudinal direction under predetermined conditions. By rapidly cooling, the heat-shrinkable polyolefin film of the present invention can be obtained. In addition, when stretching in the longitudinal direction, the gap ratio (distance from the contact point between the low-speed roll and the film to the contact point between the high-speed roll and the film when stretching in the longitudinal direction) and the film width are appropriately adjusted, so (Stretch gap / film width) can be adjusted in the range of 0.01 to 0.10.

以下、本発明の熱収縮性ポリオレフィン系フィルムを得るための好ましい二軸延伸・熱処理方法について、従来の熱収縮性ポリオレフィン系フィルムの二軸延伸・熱処理方法との差異を考慮しつつ詳細に説明する。   Hereinafter, a preferred biaxial stretching / heat treatment method for obtaining the heat-shrinkable polyolefin film of the present invention will be described in detail in consideration of the difference from the conventional biaxial stretching / heat treatment method of a heat-shrinkable polyolefin film. .

[熱収縮性ポリオレフィン系フィルムの好ましい製膜方法]
上記したように、単純に幅方向に延伸した熱収縮性フィルムは、主収縮方向と直交する方向のミシン目開封性が悪い、という不具合がある。一方、従来から長手方向に収縮する熱収縮性フィルムについての要求は高いものの、未延伸フィルムを単純に長手方向に延伸するだけでは、幅の広いフィルムが製造できないため生産性が悪い上、厚み斑の良好なフィルムを製造することができない。また、予め幅方向に延伸した後に長手方向に延伸する方法を採用すると、長手方向への収縮量が不十分となったり、幅方向に不必要に収縮するものとなってしまう。
[Preferred method for forming heat-shrinkable polyolefin film]
As described above, the heat-shrinkable film simply stretched in the width direction has a problem that the perforation opening property in the direction orthogonal to the main shrinkage direction is poor. On the other hand, although there is a high demand for a heat-shrinkable film that shrinks in the longitudinal direction, a wide film cannot be produced by simply stretching an unstretched film in the longitudinal direction. A good film cannot be produced. Moreover, if the method of extending | stretching to a longitudinal direction after extending | stretching previously to the width direction is employ | adopted, the shrinkage | contraction amount to a longitudinal direction will become inadequate, or it will shrink | contract unnecessarily in the width direction.

本発明者らは、幅方向の延伸後に長手方向に延伸する方法(以下、横−縦延伸法という)において、各延伸工程における条件によりフィルムの長手方向の温湯収縮率、ミシン目開封性、耐熱ブロッキング性がどのように変化するかについて鋭意検討した。その結果、横−縦延伸法によるフィルム製造の際に、以下の手段を講じることにより、長手方向の収縮量が高く、直交方向のミシン目開封性、耐熱ブロッキング性が良好なフィルムを安定して製造することが可能となることを突き止めた。そして、本発明者らは、それらの知見に基づいて本発明を案出するに至った。
(1)幅方向への延伸後における中間熱緩和処理
(2)長手方向へ延伸する前のフィルム端部のトリミング
以下、上記した各手段について順次説明する。
In the method of stretching in the longitudinal direction after stretching in the width direction (hereinafter referred to as the transverse-longitudinal stretching method), the inventors have performed hot water shrinkage in the longitudinal direction of the film, perforation openability, and heat resistance depending on the conditions in each stretching step. The inventors studied diligently how the blocking property changes. As a result, when the film is manufactured by the horizontal-longitudinal stretching method, the following measures are taken to stably stabilize the film having a high amount of shrinkage in the longitudinal direction and good perforation opening and heat blocking properties in the orthogonal direction. We have determined that it will be possible to manufacture. And the present inventors came to devise this invention based on those knowledge.
(1) Intermediate thermal relaxation treatment after stretching in the width direction (2) Trimming of film edge before stretching in the longitudinal direction Hereinafter, each of the above-described means will be described in order.

(1)幅方向への延伸後における中間熱緩和処理
本発明の横−縦延伸法によるフィルムの製造においては、未延伸フィルムを幅方向に延伸した後に、100℃以上155℃以下の温度で1.0秒以上50.0秒以下の時間に亘って熱処理(以下、中間熱緩和処理という)することが必要である。かかる中間熱緩和処理を行うことによって、ラベルとした場合にミシン目カット性が良好で収縮斑が生じないフィルムを得ることが可能となる。そのように横延伸後に特定の中間熱緩和処理を施すことによりミシン目カット性が良好で収縮斑が生じないフィルムを得ることが可能となる理由は明らかではないが、特定の中間熱緩和処理を施すことによって、幅方向への分子配向をある程度残存させつつ、幅方向の収縮応力を低減させることが可能となるためではないかと考えている。なお、熱緩和処理の温度の下限は、110℃以上であると好ましく、115℃以上であるとより好ましい。また、熱緩和処理の温度の上限は、150℃以下であると好ましく、145℃以下であるとより好ましい。一方、熱緩和処理の時間は、1.0秒以上50.0秒以下の範囲内で原料組成に応じて適宜調整する必要がある。
(1) Intermediate heat relaxation treatment after stretching in the width direction In the production of the film by the transverse-longitudinal stretching method of the present invention, the unstretched film is stretched in the width direction, and then at a temperature of 100 ° C to 155 ° C. It is necessary to perform heat treatment (hereinafter referred to as intermediate heat relaxation treatment) over a period of from 0.0 seconds to 50.0 seconds. By performing such an intermediate heat relaxation treatment, it is possible to obtain a film having good perforation cutability and no shrinkage spots when used as a label. The reason why it becomes possible to obtain a film having good perforation cutability and no shrinkage spots by performing a specific intermediate heat relaxation treatment after transverse stretching is not clear, but a specific intermediate heat relaxation treatment is not performed. It is thought that this can reduce the shrinkage stress in the width direction while leaving some molecular orientation in the width direction. In addition, the minimum of the temperature of a heat relaxation process is preferable in it being 110 degreeC or more, and it is more preferable in it being 115 degreeC or more. Moreover, the upper limit of the temperature of the heat relaxation treatment is preferably 150 ° C. or less, and more preferably 145 ° C. or less. On the other hand, the time for the thermal relaxation treatment needs to be appropriately adjusted in accordance with the raw material composition within a range of 1.0 second to 50.0 seconds.

また、未延伸フィルムの幅方向への延伸は、テンター内で幅方向の両端際をクリップによって把持した状態で、70℃以上140℃以下の温度で2.5倍以上8.0倍以下の倍率となるように行う必要がある。延伸温度が70℃を下回ると、延伸時に破断を起こし易くなるので好ましくなく、反対に140℃を上回ると、幅方向の厚み斑が悪くなるので好ましくない。なお、横延伸の温度の下限は、75℃以上であると好ましく、80℃以上であるとより好ましい。また、横延伸の温度の上限は、135℃以下であると好ましく、130℃以下であるとより好ましい。一方、幅方向の延伸倍率が2.5倍を下回ると、生産性が悪いばかりでなく幅方向の厚み斑が悪くなるので好ましくなく、反対に8.0倍を上回ると、延伸時に破断を起こし易くなる上、熱緩和させるのに多大なエネルギーと大掛かりな装置が必要となり、生産性が悪くなるので好ましくない。なお、横延伸の倍率の下限は、3.0倍以上であると好ましく、3.5倍以上であるとより好ましい。また、横延伸の倍率の上限は、7.5倍以下であると好ましく、7.0倍以下であるとより好ましい。   The stretching of the unstretched film in the width direction is a ratio of 2.5 times or more and 8.0 times or less at a temperature of 70 ° C. or more and 140 ° C. or less in a state where both ends of the width direction are held by clips in the tenter. It is necessary to do so. If the stretching temperature is less than 70 ° C., it is not preferable because breakage is likely to occur during stretching. On the other hand, if it exceeds 140 ° C., uneven thickness in the width direction is deteriorated, which is not preferable. The lower limit of the transverse stretching temperature is preferably 75 ° C. or higher, and more preferably 80 ° C. or higher. The upper limit of the transverse stretching temperature is preferably 135 ° C. or less, and more preferably 130 ° C. or less. On the other hand, if the draw ratio in the width direction is less than 2.5 times, not only the productivity is deteriorated but also the thickness unevenness in the width direction becomes worse. On the other hand, if it exceeds 8.0 times, breakage occurs at the time of drawing. In addition, it is not preferable because a large amount of energy and a large apparatus are required for heat relaxation, and productivity is deteriorated. In addition, the lower limit of the transverse stretching ratio is preferably 3.0 times or more, and more preferably 3.5 times or more. In addition, the upper limit of the transverse stretching ratio is preferably 7.5 times or less, and more preferably 7.0 times or less.

(2)長手方向へ延伸する前のフィルム端部のトリミング
本発明の横−縦延伸法によるフィルムの製造においては、中間熱緩和処理を施したフィルムを長手方向に延伸する前に、フィルム端縁際の十分に横延伸されていない肉厚部分(主として横延伸時のクリップ把持部分)をトリミングする必要がある。より具体的には、フィルムの左右の端縁際に位置した中央部分の厚みの約1.1〜1.3倍の厚みの部分においてカッター等の工具を用いてフィルム端縁際の肉厚部分を切断し、肉厚部分を除去しつつ、残りの部分のみを長手方向に延伸することが必要である。なお、上記の如くフィルム端部をトリミングする際には、トリミングする前のフィルムの表面温度が50℃以下となるように冷却しておくことが好ましい。そのようにフィルムを冷却することにより、切断面を乱すことなくトリミングすることが可能となる。また、フィルム端部のトリミングは、通常のカッター等を用いて行うことができるが、周状の刃先を有する丸刃を用いると、局部的に刃先が鈍くなる事態が起こらず、フィルム端部を長期間に亘ってシャープに切断し続けることができ、長手方向への延伸時における破断を誘発する事態が生じないので好ましい。
(2) Trimming of film edge before being stretched in the longitudinal direction In the production of the film by the transverse-longitudinal stretching method of the present invention, before the film subjected to the intermediate heat relaxation treatment is stretched in the longitudinal direction, the film edge It is necessary to trim a thick portion (mainly a clip gripping portion at the time of transverse stretching) that is not sufficiently transversely stretched. More specifically, a thick portion at the edge of the film using a tool such as a cutter in a portion having a thickness of about 1.1 to 1.3 times the thickness of the central portion located at the right and left edges of the film. It is necessary to stretch only the remaining part in the longitudinal direction while cutting the wall and removing the thick part. In addition, when trimming the film edge as described above, it is preferable to cool the film so that the surface temperature of the film before trimming is 50 ° C. or less. By cooling the film in this way, trimming can be performed without disturbing the cut surface. In addition, trimming of the film edge can be performed using a normal cutter or the like, but if a round blade having a circumferential cutting edge is used, a situation in which the cutting edge is locally dulled does not occur, and the film edge is This is preferable because it can continue to be cut sharply over a long period of time and does not cause a breakage during stretching in the longitudinal direction.

かかる如く、長手方向への延伸前にフィルムの端部をトリミングすることによって、一旦熱緩和処理したフィルムを均一に長手方向へ延伸することが可能となり、初めて破断のない安定したフィルムの連続製造が可能となる。加えて、長手方向(主収縮方向)の収縮量の大きなフィルムを得ることが可能となる。さらに、フィルムを均一に長手方向へ延伸することが可能となるため、長手方向の厚み斑の小さなフィルムを得ることができる。その上、フィルムの端部をトリミングすることによって、長手方向への延伸時におけるボーイングが回避され、左右の物性差の小さなフィルムを得ることが可能となる。   As described above, by trimming the end of the film before stretching in the longitudinal direction, it becomes possible to stretch the film once subjected to heat relaxation treatment uniformly in the longitudinal direction. It becomes possible. In addition, it is possible to obtain a film having a large shrinkage in the longitudinal direction (main shrinkage direction). Furthermore, since the film can be uniformly stretched in the longitudinal direction, a film having a small thickness unevenness in the longitudinal direction can be obtained. In addition, by trimming the end of the film, bowing during stretching in the longitudinal direction is avoided, and a film having a small difference in physical properties between the left and right can be obtained.

なお、上記した(1),(2)の手段の内の特定の何れかのみが、フィルムの長手方向における熱収縮性、ミシン目開封性、耐熱ブロッキング性、安定した製膜性に有効に寄与するものではなく、(1),(2)の手段を組み合わせて用いることにより、非常に効率的に、長手方向における熱収縮性、ミシン目開封性、耐熱ブロッキング性、安定した製膜性を発現させることが可能となるものと考えられる。   Note that only one of the means (1) and (2) described above contributes effectively to heat shrinkability in the longitudinal direction of the film, perforation opening, heat blocking resistance, and stable film formation. Rather than using the combination of the means (1) and (2), the heat shrinkage in the longitudinal direction, the perforation opening, the heat blocking property, and the stable film-forming property are expressed very efficiently. It is thought that it will be possible.

以下、実施例によって本発明をより詳細に説明するが、本発明は、かかる実施例の態様に何ら限定されるものではなく、本発明の趣旨を逸脱しない範囲で、適宜変更することが可能である。実施例、比較例で使用した原料の性状、組成、実施例、比較例におけるフィルムの製造条件(延伸・熱緩和処理条件等)を、それぞれ表1、表2に示す。なお、表1における樹脂原料A〜Eは、以下の通りである。
・樹脂原料A:ポリプロピレン−エチレンランダム共重合体(住友化学株式会社製 S131 エチレン=5.5質量%、MFR=1.2g/10分、融点135℃)
・樹脂原料B:ポリプロピレン−エチレンランダム共重合体(住友化学株式会社製 FS2011DG3 エチレン=0.6質量%、MFR=2.5g/10分、融点158℃)94質量%中にステアリン酸モノグリセリンエステル(帯電防止剤)6質量%を添加したもの
・樹脂原料C:ポリプロピレン−エチレンランダム共重合体(住友化学株式会社製 FS2011DG3 エチレン=0.6質量%、MFR=2.5g/10分、融点158℃)80質量%中に有機ポリマー微粒子(住友化学株式会社製 CS30 平均粒子径3.5μm)20質量%を添加したもの
・樹脂原料D:ポリプロピレン−エチレンランダム共重合体(住友化学株式会社製 FS2011DG3 エチレン=0.6質量%、MFR=2.5g/10分、融点158℃)
・樹脂原料E:ポリプロピレン−エチレン,ブテンランダム共重合体(住友化学株式会社製 FSX66E8 エチレン=2.5質量%、ブテン=6.9質量%、MFR=3.0g/10分、融点134℃)
EXAMPLES Hereinafter, the present invention will be described in more detail with reference to examples. However, the present invention is not limited to the embodiments of the examples, and can be appropriately changed without departing from the spirit of the present invention. is there. Tables 1 and 2 show properties of the raw materials used in Examples and Comparative Examples, compositions, production conditions of the films in Examples and Comparative Examples (stretching / thermal relaxation treatment conditions, etc.), respectively. In addition, resin raw material AE in Table 1 is as follows.
Resin raw material A: Polypropylene-ethylene random copolymer (Sumitomo Chemical Co., Ltd. S131 ethylene = 5.5% by mass, MFR = 1.2 g / 10 min, melting point 135 ° C.)
Resin raw material B: Polypropylene-ethylene random copolymer (FS2011DG3 ethylene = 0.6% by mass, MFR = 2.5 g / 10 min, melting point 158 ° C., manufactured by Sumitomo Chemical Co., Ltd.) 94% by mass of stearic acid monoglycerin ester (Antistatic agent) 6% by mass added; resin raw material C: polypropylene-ethylene random copolymer (FS2011DG3 ethylene = 0.6% by mass, MFR = 2.5 g / 10 min, melting point 158, manufactured by Sumitomo Chemical Co., Ltd.) ℃) Organic polymer fine particles (CS30 average particle size 3.5 μm, manufactured by Sumitomo Chemical Co., Ltd., 20% by mass) added in 80% by mass / resin raw material D: polypropylene-ethylene random copolymer (FS2011DG3 manufactured by Sumitomo Chemical Co., Ltd.) (Ethylene = 0.6 mass%, MFR = 2.5 g / 10 min, melting point 158 ° C.)
-Resin raw material E: polypropylene-ethylene, butene random copolymer (Sumitomo Chemical Co., Ltd. FSX66E8 ethylene = 2.5 mass%, butene = 6.9 mass%, MFR = 3.0 g / 10 min, melting point 134 ° C.)

Figure 0005380830
Figure 0005380830

Figure 0005380830
Figure 0005380830

また、フィルムの評価方法は下記の通りである。   Moreover, the evaluation method of a film is as follows.

[Tm(融点)]
セイコー電子工業株式会社製の示差走査熱量計(型式:DSC220)を用いて、未延伸フィルム5mgを採取し、室温より昇温速度10℃/分で昇温したときの吸熱曲線のピークの温度より求めた。
[Tm (melting point)]
Using a differential scanning calorimeter (model: DSC220) manufactured by Seiko Denshi Kogyo Co., Ltd., 5 mg of an unstretched film was sampled, and from the peak temperature of the endothermic curve when the temperature was raised from room temperature at a heating rate of 10 ° C./min. Asked.

[エチレン、ブテン含有量]
プロピレン−エチレン共重合体、プロピレン−ブテン共重合体、プロピレン−エチレン−ブテン共重合体中のエチレンあるいはブテンの含有量は、高分子分析ハンドブック(1995年、紀伊国屋書店発行)の第615〜617頁に記載された方法により、13C−NMRスペクトル法によって決定する。なお、同書の256頁「(i)ランダム共重合体」の項記載の方法によってIRスペクトル法で決定することも可能である。
[Ethylene and butene content]
The content of ethylene or butene in the propylene-ethylene copolymer, propylene-butene copolymer, and propylene-ethylene-butene copolymer is determined according to Polymer Analysis Handbook (1995, published by Kinokuniya Shoten). Determined by 13 C-NMR spectroscopy according to the method described on page. In addition, it can also be determined by the IR spectrum method according to the method described in the section “(i) Random copolymer” on page 256 of the same document.

[熱収縮率(温湯熱収縮率)]
フィルムを10cm×10cmの正方形に裁断し、所定温度(90℃)±0.5℃の温水中において、無荷重状態で10秒間処理して熱収縮させた後、フィルムの縦および横方向の寸法を測定し、上式1にしたがって、それぞれ熱収縮率を求めた。当該熱収縮率の大きい方向(長手方向)を主収縮方向とした。
[Heat shrinkage (hot water heat shrinkage)]
The film is cut into a 10 cm × 10 cm square, heat-shrinked in warm water at a predetermined temperature (90 ° C.) ± 0.5 ° C. under no load for 10 seconds, and then the vertical and horizontal dimensions of the film. Was measured, and the thermal shrinkage rate was determined according to the above formula 1. The direction (longitudinal direction) in which the heat shrinkage rate is large was defined as the main shrinkage direction.

[耐熱剥離強度]
得られたフィルム試料を2枚用意し、それらの表面同士を合わせ、テストシーラー(西部機械(株)製;シールバー幅10mm)によって90℃に加熱しながら0.4MPaの圧力を90秒加えた後、それらの重なり合った2枚のフィルムを15mm幅の短冊状に切断した。しかる後に、2枚のフィルムを、万能引張試験機((株)島津製作所製 オートグラフ)を用いて200mm/min.の条件で引き剥がしたときの剥離強度を測定した。なお、測定は5回行い、その平均値を求めた。
[Heat-resistant peel strength]
Two obtained film samples were prepared, their surfaces were combined, and a pressure of 0.4 MPa was applied for 90 seconds while heating to 90 ° C. with a test sealer (manufactured by Seibu Kikai Co., Ltd .; seal bar width 10 mm). Thereafter, the two overlapping films were cut into strips having a width of 15 mm. Thereafter, the two films were combined at 200 mm / min. Using a universal tensile tester (manufactured by Shimadzu Corporation Autograph). The peel strength when peeled off was measured. In addition, the measurement was performed 5 times and the average value was calculated | required.

[直角引裂強度]
80℃に調整された温湯中にてフィルムを主収縮方向に10%収縮させた。また、80℃で10%収縮しないフィルムについては、約5秒間に亘って80℃の温水に浸漬させることによって収縮可能な分だけ収縮させた。しかる後に、JIS−K−7128に準じて、図1に示す形状にサンプリングすることによって試験片を作製した(なお、サンプリングにおいては、試験片の長手方向をフィルムの主収縮方向とした)。しかる後に、万能引張試験機((株)島津製作所製 オートグラフ)で試験片の両端を掴み、引張速度200mm/分の条件にて、フィルムの幅方向における引張破壊時の強度の測定を行い、上式2を用いて単位厚み当たりの直角引裂強度を算出した。
[Right-angle tear strength]
The film was contracted 10% in the main contraction direction in hot water adjusted to 80 ° C. Moreover, about the film which does not shrink | contract 10% at 80 degreeC, it was made to shrink | contract only by the part which can be shrunk by being immersed in 80 degreeC warm water for about 5 seconds. Thereafter, according to JIS-K-7128, a test piece was prepared by sampling into the shape shown in FIG. 1 (in the sampling, the longitudinal direction of the test piece was set as the main shrinkage direction of the film). After that, grasp both ends of the test piece with a universal tensile tester (Autograph made by Shimadzu Corporation), and measure the strength at the time of tensile fracture in the width direction of the film under the condition of a tensile speed of 200 mm / min. The right angle tear strength per unit thickness was calculated using Equation 2 above.

[エルメンドルフ比]
得られたフィルムを矩形状の枠に予め弛ませた状態で装着し(フィルムの両端を枠によって把持させ)、弛んだフィルムが枠内で緊張状態となるまで(弛みがなくなるまで)、約5秒間に亘って80℃の温水に浸漬させることによって、フィルムを主収縮方向に10%収縮させた(以下、予備収縮という)。また、80℃で10%収縮しないフィルムについては、約5秒間に亘って80℃の温水に浸漬させることによって収縮可能な分だけ収縮させた。しかる後に、JIS−K−7128に準じて、主収縮方向×直交方向=63mm×75mmのサイズに切り取り、長尺な端縁(直交方向に沿った端縁)の中央から当該端縁に直交するように20mmのスリット(切り込み)を入れることによって試験片を作製した。そして、作製された試験片を用いて主収縮方向のエルメンドルフ引裂荷重の測定を行った。また、上記方法と同様な方法でフィルムを主収縮方向に予備収縮させた後に、フィルムの主収縮方向と直交方向とを入れ替えて試験片を作製し、直交方向のエルメンドルフ引裂荷重の測定を行った。そして、得られた主収縮方向および主収縮方向と直交する方向のエルメンドルフ引裂荷重から上式3を用いてエルメンドルフ比を算出した。
[Elmendorf ratio]
The obtained film is attached to a rectangular frame in a state of being loosened in advance (with both ends of the film being gripped by the frame), and until the loose film is in a tension state within the frame (until loosening), about 5 The film was shrunk by 10% in the main shrinking direction (hereinafter referred to as pre-shrinking) by immersing in warm water at 80 ° C. for 2 seconds. Moreover, about the film which does not shrink | contract 10% at 80 degreeC, it was made to shrink | contract only by the part which can be shrunk by being immersed in 80 degreeC warm water for about 5 seconds. After that, in accordance with JIS-K-7128, the main shrinkage direction × orthogonal direction = 63 mm × 75 mm is cut out and perpendicular to the edge from the center of the long edge (edge along the orthogonal direction). Thus, the test piece was produced by putting a 20 mm slit (cut). And the Elmendorf tear load of the main contraction direction was measured using the produced test piece. Further, after preliminarily shrinking the film in the main shrinkage direction by the same method as described above, a test piece was prepared by replacing the main shrinkage direction and the orthogonal direction of the film, and the Elmendorf tear load in the orthogonal direction was measured. . Then, the Elmendorf ratio was calculated from the obtained main contraction direction and the Elmendorf tear load in the direction orthogonal to the main contraction direction using the above equation 3.

[収縮仕上り性]
主収縮方向が長手方向のフィルムロールについては、得られたフィルムロールを、約120mmの幅にスリットした上で、所定の長さに分割して巻き取ることによって小型のスリットロールを作成し、そのスリットロールに、予め東洋インキ製造(株)の草色・金色・白色のインキを用いて、ラベル用の印刷(3色印刷)を繰り返し施した。また、各ラベル用印刷毎に、フィルムロールの長手方向と直交する方向に、フィルム全幅に亘るミシン目(約1mm間隔で約1mm径の円が連続するミシン目)を、約22mmの間隔で2本平行に形成した。そして、ラベル用の印刷が施されたロール状のフィルムの片方の端部を、350mlの角型ホット用PETボトル(中身を充填したもの)の外周の一部に塗布した粘着剤の上に重ねることによって接着し、その状態で、ロール状のフィルムを所定の長さだけ引き出して、PETボトルの外周に捲回させた。しかる後、PETボトルの外周で重なり合った熱収縮性フィルム同士を上記した粘着剤によって貼り合わせながら、カッターにより外側のフィルムを鉛直方向に切断することによって、PETボトルの外周にラベルを被覆させた。
[Shrink finish]
For a film roll whose main shrinkage direction is the longitudinal direction, the obtained film roll is slit into a width of about 120 mm, and then a small slit roll is created by winding it into a predetermined length, Label printing (three-color printing) was repeatedly applied to the slit roll in advance using grass-colored, gold-colored, and white inks from Toyo Ink Manufacturing Co., Ltd. For each label printing, perforations over the entire width of the film (perforations in which circles of about 1 mm in diameter are continuous at intervals of about 1 mm) in a direction perpendicular to the longitudinal direction of the film roll are provided at intervals of about 22 mm. These were formed in parallel. Then, one end of the roll-shaped film on which the label printing is applied is overlaid on the adhesive applied to a part of the outer periphery of a 350 ml square hot PET bottle (filled with the contents). In this state, the roll-shaped film was drawn out by a predetermined length and wound around the outer periphery of the PET bottle. Thereafter, while the heat-shrinkable films overlapped on the outer periphery of the PET bottle were bonded to each other with the above-mentioned adhesive, the outer film was cut in the vertical direction with a cutter to coat the outer periphery of the PET bottle.

一方、主収縮方向が幅方向のフィルムロールについては、熱収縮性フィルムに、予め東洋インキ製造(株)の草色・金色・白色のインキで3色印刷を施した。そして、印刷したフィルムの両端部を白光株式会社製、白光シーラー(型式:No.310−1)でヒートシールすることにより、円筒状のラベルを作成した。しかる後、作成されたラベルをPETボトルの周囲に装着した。   On the other hand, for the film roll whose main shrinkage direction is the width direction, the heat-shrinkable film was preliminarily printed with three colors with grass-colored, gold-colored, and white inks from Toyo Ink Manufacturing Co., Ltd. And the cylindrical label was created by heat-sealing the both ends of the printed film with a white light sealer (model: No. 310-1) by Hakuko Co., Ltd. Thereafter, the produced label was attached around the PET bottle.

そして、Fuji Astec Inc製スチームトンネル(型式;SH−1500−L)を用い、ラベルを被覆させたPETボトル(長手方向が主収縮方向であるフィルムからなるラベルを被覆させたPETボトル、および、幅方向が主収縮方向であるフィルムからなるラベルを被覆させたPETボトル)を、通過時間10秒、ゾーン温度80℃の条件下で通過させ、PETボトルの外周においてラベルを熱収縮させることによってラベルの装着を完了した。なお、装着の際には、ネック部においては、直径40mmの部分がラベルの一方の端になるように調整した。収縮後の仕上がり性の評価は目視で行い、基準は下記の通りとした。
◎:シワ,飛び上り、収縮不足の何れも未発生で、かつ色の斑も見られない
○:シワ,飛び上り、または収縮不足が確認できないが、若干、色の斑が見られる
△:飛び上り、収縮不足の何れも未発生だが、ネック部の斑が見られる
×:シワ、飛び上り、収縮不足が発生
Then, using a steam tunnel (model: SH-1500-L) manufactured by Fuji Astec Inc, a PET bottle coated with a label (a PET bottle coated with a label made of a film whose longitudinal direction is the main shrinkage direction, and width) The PET bottle coated with a label made of a film whose direction is the main shrinkage direction) is passed under conditions of a passage time of 10 seconds and a zone temperature of 80 ° C., and the label is thermally shrunk on the outer periphery of the PET bottle. Completed installation. At the time of mounting, the neck portion was adjusted so that a portion with a diameter of 40 mm was one end of the label. The finish after shrinkage was evaluated visually, and the criteria were as follows.
◎: No wrinkles, jumping up, insufficient shrinkage, and no color spots are observed ○: Wrinkles, jumping up, or insufficient shrinkage cannot be confirmed, but some color spots are seen △: Jumping Neither ascending nor insufficient shrinkage has occurred, but spots on the neck are observed. ×: Wrinkles, jumping up, insufficient shrinkage occurred

[ミシン目開封性]
予め主収縮方向とは直交する方向にミシン目を入れておいたラベルを、上記した収縮仕上り性の測定条件と同一の条件でPETボトルに装着した。ただし、ミシン目は、長さ1mmの孔を1mm間隔で入れることによって形成し、ラベルの縦方向(高さ方向)に幅22mm、長さ120mmに亘って2本設けた。その後、このボトルを5℃で冷蔵し、冷蔵庫から取り出した直後のボトルのラベルのミシン目を指先で引裂き、縦方向にミシン目に沿って綺麗に裂け、ラベルをボトルから外すことができた本数を数え、全サンプル50本に対する割合(%)を算出した。
[Perforation opening]
A label having perforations in a direction perpendicular to the main shrinkage direction was attached to the PET bottle under the same conditions as the measurement conditions for shrinkage finish described above. However, the perforations were formed by putting holes having a length of 1 mm at intervals of 1 mm, and two perforations were provided in the longitudinal direction (height direction) of the label over a width of 22 mm and a length of 120 mm. The bottle was then refrigerated at 5 ° C, and the bottle label perforation immediately after removal from the refrigerator was torn with the fingertips. And the ratio (%) with respect to all 50 samples was calculated.

[耐熱ブロッキング性]
上記した収縮仕上り性の評価時と同様の方法で、350mlの角型ホット用PETボトル飲料(中身を充填したもの)の外周に、熱収縮性フィルムを熱収縮させて装着した。そして、同様な熱収縮性フィルムの装着を施したPETボトル飲料5個を、鉛直に積み上げ、70℃の条件下で5日間放置した後に、PETボトル飲料の外面のフィルム同士にブロッキングがあるか否かを下記の2段階で官能評価した(なお、わずかでもブロッキングが認められる場合は×とした)。
○・・ブロッキングなし
×・・ブロッキングあり
[Heat-resistant blocking property]
A heat-shrinkable film was heat-shrinked and mounted on the outer periphery of a 350 ml square hot PET bottle beverage (filled with contents) in the same manner as in the evaluation of the shrink finish. And after five PET bottle drinks which attached the same heat-shrinkable film were piled up vertically and left to stand on 70 degreeC conditions for 5 days, whether there is blocking between the films of the outer surface of PET bottle drinks? These were subjected to sensory evaluation in the following two stages (note that even a slight blocking was indicated as x).
○ ・ ・ No blocking × ・ ・ With blocking

[実施例1]
共押出法を利用して、2つの押出機(第一,第二押出機)からポリオレフィン系樹脂を溶融押出し(ダイス内で積層して押出し)し、30℃に冷却された回転する金属ロールに巻き付けて急冷することにより、厚さが400μmで二種三層構成の未延伸フィルム(ポリオレフィン系樹脂積層シート)を得た。このときの未延伸フィルムの引取速度(金属ロールの回転速度)は、約6.8m/min.であった。未延伸フィルムの各層の形成方法(溶融押出までの工程)は、以下の通りである。なお、以下の説明においては、ポリオレフィン系樹脂積層シートの表層から順に、第一層、第二層、第三層という(すなわち、第三層の表面は、金属ロール接触面である)。なお、未延伸フィルムの形成における第一,第二押出機の吐出量は、第一層/第二層/第三層の厚み比が、1/4/1となるように調整した。
[Example 1]
Using a co-extrusion method, a polyolefin resin is melt-extruded (laminated in a die and extruded) from two extruders (first and second extruders) into a rotating metal roll cooled to 30 ° C. By winding and quenching, an unstretched film (polyolefin-based resin laminated sheet) having a thickness of 400 μm and a two-layer / three-layer structure was obtained. At this time, the take-up speed of the unstretched film (rotational speed of the metal roll) is about 6.8 m / min. Met. The method for forming each layer of the unstretched film (steps until melt extrusion) is as follows. In the following description, the first layer, the second layer, and the third layer are referred to in order from the surface layer of the polyolefin-based resin laminate sheet (that is, the surface of the third layer is a metal roll contact surface). In addition, the discharge amount of the 1st, 2nd extruder in formation of an unstretched film was adjusted so that the thickness ratio of 1st layer / 2nd layer / 3rd layer might become 1/4/1.

・第一層および第三層(スキン層)の形成
乾燥させた上記原料樹脂A,B,Cを、押出機(第一押出機)のホッパに、定量スクリューフィーダーで連続的に別々に供給した。なお、原料樹脂Aの供給量を90質量%とし、原料樹脂Bの供給量を8質量%とし、原料樹脂Cの供給量を2質量%とした。そして、供給された原料樹脂A,B,Cを、ホッパ内で混合し、単軸式の第一押出機により250℃でTダイから溶融押出しした。
Formation of the first layer and the third layer (skin layer) The dried raw material resins A, B, and C were continuously and separately supplied to the hopper of the extruder (first extruder) with a quantitative screw feeder. . The supply amount of the raw material resin A was 90% by mass, the supply amount of the raw material resin B was 8% by mass, and the supply amount of the raw material resin C was 2% by mass. Then, the supplied raw material resins A, B, and C were mixed in a hopper and melt-extruded from a T die at 250 ° C. by a single-screw first extruder.

・第二層(コア層)の形成
乾燥させた上記原料樹脂Aを、押出機(第二押出機)のホッパに、定量スクリューフィーダーで連続的に別々に供給した。そして、供給された原料樹脂Aを、単軸式の第二押出機により250℃でTダイから溶融押出しした。
-Formation of 2nd layer (core layer) The dried said raw material resin A was continuously supplied separately to the hopper of the extruder (2nd extruder) with the fixed amount screw feeder. The supplied raw material resin A was melt-extruded from a T die at 250 ° C. by a single-screw second extruder.

しかる後、得られた未延伸フィルムを、横延伸ゾーン、中間ゾーン、中間熱緩和処理ゾーンを連続的に設けたテンターに導いた。なお、当該テンターにおいては、横延伸ゾーンと中間熱緩和処理ゾーンとの中間に位置した中間ゾーンの長さが、約40cmに設定されている。また、中間ゾーンにおいては、フィルムを通過させていない状態で短冊状の紙片を垂らしたときに、その紙片がほぼ完全に鉛直方向に垂れ下がるように、延伸ゾーンからの熱風および熱処理ゾーンからの熱風が遮断されている。   Thereafter, the obtained unstretched film was guided to a tenter in which a transverse stretching zone, an intermediate zone, and an intermediate heat relaxation treatment zone were continuously provided. In the tenter, the length of the intermediate zone located between the transverse stretching zone and the intermediate thermal relaxation treatment zone is set to about 40 cm. In addition, in the intermediate zone, when the strip-shaped paper piece is hung in a state where the film is not passed through, the hot air from the stretching zone and the hot air from the heat treatment zone are blown so that the paper piece hangs almost completely in the vertical direction. Blocked.

そして、テンターに導かれた未延伸フィルムを、フィルム温度が89℃になるまで予備加熱した後、横延伸ゾーンで横方向に89℃で4.5倍に延伸し、中間ゾーンを通過させた後に、中間熱緩和処理ゾーンへ導き、145℃の温度で43秒間に亘って熱処理することによって厚み90μmの横一軸延伸フィルムを得た。しかる後、テンターの後方に設けられた左右一対のトリミング装置(周状の刃先を有する丸刃によって構成されたもの)を利用して、横一軸延伸フィルムの端縁際(中央のフィルム厚みの約1.2倍の厚みの部分)を切断し、切断部位の外側に位置したフィルムの端部を連続的に除去した。   And after preheating the unstretched film led to the tenter until the film temperature reaches 89 ° C., it is stretched 4.5 times at 89 ° C. in the transverse direction in the transverse stretching zone, and after passing through the intermediate zone Then, the film was led to an intermediate heat relaxation treatment zone and heat treated at a temperature of 145 ° C. for 43 seconds to obtain a transversely uniaxially stretched film having a thickness of 90 μm. Thereafter, using a pair of left and right trimming devices (configured by a round blade having a circumferential cutting edge) provided behind the tenter, the edge of the laterally uniaxially stretched film (about the thickness of the film at the center) A portion having a thickness of 1.2 times) was cut, and the end portion of the film located outside the cut site was continuously removed.

さらに、そのように端部をトリミングしたフィルム(フィルム幅=500mm)を、複数のロール群を連続的に配置した縦延伸機へ導き、予熱ロール上でフィルム温度が90℃になるまで予備加熱した後に、表面温度100℃に設定された低速延伸ロールと内部の循環水の温度が30℃に設定された高速延伸ロールとの間で2.0倍に延伸した。なお、低速ロールの速度(低速ロールとともに移動するフィルムの速度)は、3.0m/min.に調整し、高速ロールの速度(高速ロールとともに移動するフィルムの速度)は、6.0m/min.に調整した。また、低速延伸ロールと高速延伸ロールとの延伸ギャップは30mmに調整した(延伸ギャップ比率=0.06)。   Furthermore, the film (film width = 500 mm) with the end trimmed as described above was led to a longitudinal stretching machine in which a plurality of roll groups were continuously arranged, and preheated until the film temperature reached 90 ° C. on the preheating roll. Later, the film was stretched 2.0 times between a low-speed stretching roll whose surface temperature was set to 100 ° C. and a high-speed stretching roll whose internal circulating water temperature was set to 30 ° C. The speed of the low-speed roll (the speed of the film moving with the low-speed roll) is 3.0 m / min. The speed of the high-speed roll (the speed of the film that moves with the high-speed roll) is 6.0 m / min. Adjusted. The stretching gap between the low-speed stretching roll and the high-speed stretching roll was adjusted to 30 mm (stretching gap ratio = 0.06).

そして、上記の如く縦延伸した後のフィルムを紙管に巻き取ることによって、約50μmの二軸延伸フィルム(熱収縮性ポリオレフィンフィルム)を所定の長さだけ捲回したフィルムロールを得た。そして、得られたフィルムの特性を上記した方法によって評価した。評価結果を表3に示す。   And the film roll which wound the biaxially stretched film (heat-shrinkable polyolefin film) of about 50 micrometers by predetermined length by winding up the film after extending | stretching longitudinally as mentioned above to a paper tube was obtained. And the characteristic of the obtained film was evaluated by the above-mentioned method. The evaluation results are shown in Table 3.

[実施例2]
縦延伸する際の低速延伸ロールの表面温度を110℃に設定した以外は、実施例1と同様の方法によって、熱収縮性フィルムを捲回したフィルムロールを得た。そして、得られたフィルムの特性を実施例1と同様の方法によって評価した。評価結果を表3に示す。
[Example 2]
A film roll wound with a heat-shrinkable film was obtained in the same manner as in Example 1 except that the surface temperature of the low-speed stretching roll during longitudinal stretching was set to 110 ° C. And the characteristic of the obtained film was evaluated by the same method as Example 1. The evaluation results are shown in Table 3.

[実施例3]
縦延伸する際の高速ロールの速度を15.0m/min.に調整した(縦延伸倍率=5.0倍)以外は、実施例2と同様の方法によって、厚み約20μmの熱収縮性フィルムを捲回したフィルムロールを得た。そして、得られたフィルムの特性を実施例1と同様の方法によって評価した。評価結果を表3に示す。
[Example 3]
The speed of the high-speed roll during longitudinal stretching is 15.0 m / min. A film roll obtained by winding a heat-shrinkable film having a thickness of about 20 μm was obtained in the same manner as in Example 2 except that the film was adjusted to (longitudinal stretch ratio = 5.0 times). And the characteristic of the obtained film was evaluated by the same method as Example 1. The evaluation results are shown in Table 3.

[実施例4]
縦延伸する際の低速延伸ロールの表面温度を110℃に設定し、かつ高速ロールの速度を10.5m/min.に調整した(縦延伸倍率=3.5倍)以外は、実施例1と同様の方法によって、厚み約30μmの熱収縮性フィルムを捲回したフィルムロールを得た。そして、得られたフィルムの特性を実施例1と同様の方法によって評価した。評価結果を表3に示す。
[Example 4]
The surface temperature of the low-speed stretching roll during longitudinal stretching is set to 110 ° C., and the speed of the high-speed roll is set to 10.5 m / min. A film roll obtained by winding a heat-shrinkable film having a thickness of about 30 μm was obtained in the same manner as in Example 1 except that the film was adjusted to (longitudinal stretch ratio = 3.5 times). And the characteristic of the obtained film was evaluated by the same method as Example 1. The evaluation results are shown in Table 3.

[実施例5]
コア層を形成する樹脂原料を樹脂原料Eに変更した以外は、実施例4と同様の方法によって、熱収縮性フィルムを捲回したフィルムロールを得た。そして、得られたフィルムの特性を実施例1と同様の方法によって評価した。評価結果を表3に示す。
[Example 5]
A film roll wound with a heat-shrinkable film was obtained in the same manner as in Example 4 except that the resin raw material for forming the core layer was changed to the resin raw material E. And the characteristic of the obtained film was evaluated by the same method as Example 1. The evaluation results are shown in Table 3.

[実施例6]
縦延伸する際の高速ロールの速度を9.0m/min.に調整した(縦延伸倍率=3.0倍)以外は、実施例4と同様の方法によって、厚み約36μmの熱収縮性フィルムを捲回したフィルムロールを得た。そして、得られたフィルムの特性を実施例1と同様の方法によって評価した。評価結果を表3に示す。
[Example 6]
The speed of the high-speed roll during longitudinal stretching is 9.0 m / min. A film roll obtained by winding a heat-shrinkable film having a thickness of about 36 μm was obtained in the same manner as in Example 4 except that the film was adjusted to (longitudinal stretch ratio = 3.0 times). And the characteristic of the obtained film was evaluated by the same method as Example 1. The evaluation results are shown in Table 3.

[実施例7]
未延伸の樹脂シートを形成する際に、第二押出機に供給する樹脂原料を表1の如く変更するとともに、第一層および第三層を形成することなく第二層のみの単層構造とした以外は、実施例4と同様の方法によって、厚み約30μmの熱収縮性フィルムを捲回したフィルムロールを得た。そして、得られたフィルムの特性を実施例1と同様の方法によって評価した。評価結果を表3に示す。
[Example 7]
When forming an unstretched resin sheet, the resin raw material supplied to the second extruder is changed as shown in Table 1, and a single-layer structure of only the second layer without forming the first layer and the third layer. The film roll which wound the heat-shrinkable film about 30 micrometers thick was obtained by the method similar to Example 4 except having performed. And the characteristic of the obtained film was evaluated by the same method as Example 1. The evaluation results are shown in Table 3.

[比較例1]
二種三層構成の未延伸フィルムの厚みを110μmとし、中間熱緩和処理の温度を70℃に変更し、縦延伸を行わなかった以外は、実施例1と同様の方法で厚み約24μmの熱収縮性フィルムを捲回したフィルムロールを得た。そして、得られたフィルムの特性を実施例1と同様の方法によって評価した。評価結果を表3に示す。
[Comparative Example 1]
A heat of about 24 μm in thickness is obtained in the same manner as in Example 1 except that the thickness of the unstretched film of the two-layer / three-layer configuration is 110 μm, the temperature of the intermediate heat relaxation treatment is changed to 70 ° C., and no longitudinal stretching is performed A film roll wound with a shrinkable film was obtained. And the characteristic of the obtained film was evaluated by the same method as Example 1. The evaluation results are shown in Table 3.

[比較例2]
二種三層構成の未延伸フィルムの厚みを110μmとし、横延伸、中間熱緩和処理することなく縦延伸機に未延伸フィルムを導き、縦延伸における低速ロールの速度を1.0m/min.に変更し、高速ロールの速度を6.0m/min.(縦延伸倍率=6.0倍)に変更した以外は、実施例1と同様の方法で縦延伸することによって、厚み約20μmの熱収縮性フィルムを捲回したフィルムロールを得た。そして、得られたフィルムの特性を実施例1と同様の方法によって評価した。評価結果を表3に示す。
[Comparative Example 2]
The unstretched film having a two-layer / three-layer structure has a thickness of 110 μm, and the unstretched film is guided to the longitudinal stretching machine without undergoing transverse stretching and intermediate heat relaxation treatment, and the speed of the low-speed roll in the longitudinal stretching is 1.0 m / min. And the speed of the high-speed roll was changed to 6.0 m / min. A film roll obtained by winding a heat-shrinkable film having a thickness of about 20 μm was obtained by longitudinal stretching in the same manner as in Example 1 except that the ratio was changed to (longitudinal stretching ratio = 6.0 times). And the characteristic of the obtained film was evaluated by the same method as Example 1. The evaluation results are shown in Table 3.

[比較例3]
スキン層、コア層を形成する樹脂原料およびその組成を表1の如く変更するとともに、縦延伸を行わなかった以外は、実施例1と同様の方法によって熱収縮性フィルムを捲回したフィルムロールを得ようと試みたが、横延伸の工程で破断を頻発したため、評価し得るフィルムを得ることができなかった。
[Comparative Example 3]
A film roll in which a heat-shrinkable film was wound by the same method as in Example 1 except that the resin raw material for forming the skin layer and the core layer and the composition thereof were changed as shown in Table 1, and longitudinal stretching was not performed. Although it tried to obtain, since the breakage occurred frequently in the step of transverse stretching, a film that could be evaluated could not be obtained.

[比較例4]
スキン層、コア層を形成する樹脂原料およびその組成を表1の如く変更するとともに、中間熱緩和処理の温度を160℃に変更し、縦延伸する際の低速ロールの温度を140℃に変更した以外は、実施例4と同様の方法によって、厚み約30μmの熱収縮性フィルムを捲回したフィルムロールを得た。そして、得られたフィルムの特性を実施例1と同様の方法によって評価した。評価結果を表3に示す。
[Comparative Example 4]
The resin raw material for forming the skin layer and the core layer and the composition thereof were changed as shown in Table 1, the temperature of the intermediate heat relaxation treatment was changed to 160 ° C., and the temperature of the low-speed roll during longitudinal stretching was changed to 140 ° C. The film roll which wound the heat-shrinkable film about 30 micrometers thick by the method similar to Example 4 was obtained. And the characteristic of the obtained film was evaluated by the same method as Example 1. The evaluation results are shown in Table 3.

Figure 0005380830
Figure 0005380830

表3から明らかなように、実施例1〜7で得られたフィルムは、いずれも、主収縮方向である長手方向への収縮性が高く、主収縮方向と直交する幅方向への収縮性は非常に低かった。また、実施例1〜7で得られたフィルムは、いずれも、耐熱剥離強度が低く、収縮斑もなく、収縮仕上がり性、ミシン目開封性、耐熱ブロッキング性が良好であった。すなわち、実施例で得られた熱収縮性ポリオレフィン系フィルムは、いずれもラベルとしての品質が高く、きわめて実用性の高いものであった。   As is clear from Table 3, the films obtained in Examples 1 to 7 all have high shrinkability in the longitudinal direction, which is the main shrinkage direction, and the shrinkage in the width direction orthogonal to the main shrinkage direction is It was very low. Moreover, all of the films obtained in Examples 1 to 7 had low heat-resistant peel strength, no shrinkage spots, and good shrinkage finish, perforation openability, and heat-resistant blocking properties. That is, the heat-shrinkable polyolefin films obtained in the examples were all high in label quality and extremely practical.

それに対して、比較例1,2で得られた熱収縮性フィルムは、ミシン目開封性が不良であった。また、比較例3の条件では、評価し得るフィルムを得ることができなかった。さらに、比較例4で得られたフィルムは、長手方向の熱収縮率がきわめて低く、ラベルとして装着させた際に収縮不足のためうまく装着ができず、ミシン目開封性、耐熱ブロッキング性を評価し得るラベル付きボトルを得ることができなかった。すなわち、比較例で得られた熱収縮性ポリオレフィン系フィルムは、いずれもラベルとしての品質に劣り、実用性の低いものであった。   On the other hand, the heat-shrinkable films obtained in Comparative Examples 1 and 2 had poor perforation openability. Moreover, the film which can be evaluated was not able to be obtained on the conditions of the comparative example 3. Furthermore, the film obtained in Comparative Example 4 has a very low heat shrinkage rate in the longitudinal direction, and when mounted as a label, it cannot be mounted well due to insufficient shrinkage, and was evaluated for perforation opening and heat blocking resistance. Could not get a labeled bottle to get. That is, the heat-shrinkable polyolefin film obtained in the comparative example was inferior in quality as a label and low in practicality.

本発明の熱収縮性ポリオレフィン系フィルムは、上記の如く優れた加工特性を有しているので、ボトルのラベル用途に好適に用いることができる。   Since the heat-shrinkable polyolefin film of the present invention has excellent processing characteristics as described above, it can be suitably used for labeling bottles.

直角引裂強度の測定における試験片の形状を示す説明図である(なお、図中における試験片の各部分の長さの単位はmmである)。It is explanatory drawing which shows the shape of the test piece in the measurement of a right-angled tear strength (In addition, the unit of the length of each part of the test piece in a figure is mm).

符号の説明Explanation of symbols

F・・フィルム。   F ・ ・ Film.

Claims (6)

プロピレン−α−オレフィン共重合体を主成分とするポリオレフィン系樹脂によって一定幅の長尺状に形成されており、主収縮方向が長手方向である熱収縮性ポリオレフィン系フィルムであって、脂肪酸アルキルアミン、脂肪酸アルキルアミンエステル、脂肪酸モノグリセリンエステルから選ばれる界面活性剤の帯電防止剤が添加されており、下記要件(1)〜(4)を満たすことを特徴とする熱収縮性ポリオレフィン系フィルム。
(1)90℃の温水中で10秒間に亘って処理した場合における長手方向の温湯熱収縮率が15%以上40%以下であること
(2)90℃の温水中で10秒間に亘って処理した場合における長手方向と直交する幅方向の温湯熱収縮率が−5%以上10%以下であること
(3)80℃の温水中で長手方向に10%収縮させた後の単位厚み当たりの幅方向の直角引裂強度が50N/mm以上200N/mm以下であること
(4)フィルムの表面同士を合わせて90℃に加熱しながら0.4MPaの圧力を90秒間加えたときの剥離強度が0.1N/15mm以下であること
A heat-shrinkable polyolefin-based film which is formed in a long shape with a certain width by a polyolefin-based resin containing a propylene-α-olefin copolymer as a main component and whose main shrinkage direction is the longitudinal direction, and is a fatty acid alkylamine A heat-shrinkable polyolefin film, wherein a surfactant antistatic agent selected from fatty acid alkylamine esters and fatty acid monoglycerin esters is added, and satisfies the following requirements (1) to (4).
(1) The hot water heat shrinkage in the longitudinal direction is 15% or more and 40% or less when treated in 90 ° C. warm water for 10 seconds. (2) Treated in 90 ° C. warm water for 10 seconds. The hot-water heat shrinkage rate in the width direction perpendicular to the longitudinal direction is -5% to 10%. (3) Width per unit thickness after shrinking 10% in the longitudinal direction in hot water at 80 ° C The perpendicular tear strength in the direction is 50 N / mm or more and 200 N / mm or less. (4) The peel strength when a pressure of 0.4 MPa is applied for 90 seconds while the surfaces of the films are combined and heated to 90 ° C. is 0. 1N / 15mm or less
ポリオレフィン系樹脂が、プロピレンとエチレンとの共重合体を主成分とするものであり、構成樹脂中のエチレンの量が、2.0質量%以上10.0質量%以下であることを特徴とする請求項1に記載の熱収縮性ポリオレフィン系フィルム。 The polyolefin resin is mainly composed of a copolymer of propylene and ethylene, and the amount of ethylene in the constituent resin is 2.0% by mass or more and 10.0% by mass or less. The heat-shrinkable polyolefin film according to claim 1. ポリオレフィン系樹脂が、プロピレンとエチレンとブテンとの共重合体を主成分とするものであり、構成樹脂中のエチレンおよびブテンの量が、3.0質量%以上10.0質量%以下であることを特徴とする請求項1に記載の熱収縮性ポリオレフィン系フィルム。 The polyolefin-based resin is mainly composed of a copolymer of propylene, ethylene and butene, and the amount of ethylene and butene in the constituent resin is 3.0% by mass or more and 10.0% by mass or less. The heat-shrinkable polyolefin film according to claim 1. ポリオレフィン系樹脂が、プロピレンとブテンとの共重合体を主成分とするものであり、構成樹脂中のブテンの量が、15.0質量%以上35.0質量%以下であることを特徴とする請求項1に記載の熱収縮性ポリオレフィン系フィルム。 The polyolefin-based resin is mainly composed of a copolymer of propylene and butene, and the amount of butene in the constituent resin is 15.0% by mass or more and 35.0% by mass or less. The heat-shrinkable polyolefin film according to claim 1. コア層の少なくとも片面にスキン層を積層した積層構造を有しており、前記スキン層中に、アンチブロッキング剤および/または脂肪酸アルキルアミン、脂肪酸アルキルアミンエステル、脂肪酸モノグリセリンエステルから選ばれる界面活性剤の帯電防止剤が添加されていることを特徴とする請求項1〜4のいずれかに記載の熱収縮性ポリオレフィン系フィルム。 A surfactant having a laminated structure in which a skin layer is laminated on at least one side of the core layer, and an antiblocking agent and / or a surfactant selected from a fatty acid alkylamine, a fatty acid alkylamine ester, and a fatty acid monoglycerin ester in the skin layer The heat-shrinkable polyolefin film according to any one of claims 1 to 4, wherein an antistatic agent is added. 請求項1〜5のいずれかに記載の熱収縮性ポリオレフィン系フィルムを製造するための製造方法であって、
未延伸フィルムを、テンター内で幅方向の両端際をクリップによって把持した状態で70℃以上140℃以下の温度で幅方向に2.5倍以上8.0倍以下の倍率で延伸した後に、100℃以上155℃以下の温度で1.0秒以上50.0秒以下の時間に亘って熱緩和処理し、しかる後、フィルムの幅方向の両端縁のクリップ把持部分を切断除去した後、70℃以上140℃以下の温度で長手方向に2.0倍以上8.0倍以下の倍率で延伸することを特徴とする熱収縮性ポリオレフィン系フィルムの製造方法。
A production method for producing the heat-shrinkable polyolefin film according to claim 1,
The unstretched film is stretched at a magnification of 2.5 to 8.0 times in the width direction at a temperature of 70 ° C. or more and 140 ° C. or less with the clip held at both ends in the width direction in the tenter, and then 100 Heat relaxation treatment at a temperature not lower than 155 ° C. and lower than 155 ° C. for a time not shorter than 1.0 second and not longer than 50.0 seconds, and then cuts and removes clip holding portions at both edges in the width direction of the film, and then 70 ° C. A method for producing a heat-shrinkable polyolefin film, wherein the film is stretched at a temperature of 140 ° C. or less at a magnification of 2.0 times or more and 8.0 times or less in the longitudinal direction.
JP2007315497A 2006-12-20 2007-12-06 Heat-shrinkable polyolefin film and method for producing the same Active JP5380830B2 (en)