JP3675493B2 - Flame retardant resin composition - Google Patents

Flame retardant resin composition Download PDF

Info

Publication number
JP3675493B2
JP3675493B2 JP35353293A JP35353293A JP3675493B2 JP 3675493 B2 JP3675493 B2 JP 3675493B2 JP 35353293 A JP35353293 A JP 35353293A JP 35353293 A JP35353293 A JP 35353293A JP 3675493 B2 JP3675493 B2 JP 3675493B2
Authority
JP
Japan
Prior art keywords
weight
component
formula
parts
resin
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Lifetime
Application number
JP35353293A
Other languages
Japanese (ja)
Other versions
JPH07196873A (en
Inventor
智英 藤口
明宏 斉藤
秀行 糸井
Original Assignee
日本ジーイープラスチックス株式会社
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Family has litigation
First worldwide family litigation filed litigation Critical https://patents.darts-ip.com/?family=18431476&utm_source=google_patent&utm_medium=platform_link&utm_campaign=public_patent_search&patent=JP3675493(B2) "Global patent litigation dataset” by Darts-ip is licensed under a Creative Commons Attribution 4.0 International License.
Application filed by 日本ジーイープラスチックス株式会社 filed Critical 日本ジーイープラスチックス株式会社
Priority to JP35353293A priority Critical patent/JP3675493B2/en
Publication of JPH07196873A publication Critical patent/JPH07196873A/en
Application granted granted Critical
Publication of JP3675493B2 publication Critical patent/JP3675493B2/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Description

【0001】
【産業上の利用分野】
本発明は、ポリカーボネート系の樹脂を含む難燃化された樹脂組成物に関する。
【0002】
【従来の技術および発明が解決しようとする課題】
ポリカーボネート樹脂は、耐熱性、耐衝撃性等に優れることから種々の用途に用いられているが、成形加工温度が高く、流動性が悪いこと、衝撃強度の厚み依存性が大きい等の欠点を有している。
【0003】
そこで、ポリカーボネート(PC)樹脂にABS(アクリロニトリル‐ブタジエン‐スチレン)系樹脂をブレンドし、これらの問題点を解決しようとする試みがなされている(特公昭38-15225号公報、特公昭48-12170号公報、特公昭57-21530号公報、特公昭58-46269号公報等)。
【0004】
ところでPC/ABSアロイは、成形加工性、耐衝撃性に優れるが、難燃性が不足しているため、難燃性向上のために種々の試みが成されている(特公昭54-30417公報、特開昭61-62556号公報)。
【0005】
しかしながら、近年機器のコストダウンや軽量化の要請に伴い、薄肉化指向が強まりつつある。材料においても、薄肉化を達成するため、例えばポリカーボネートの分子量を低くしたり、ABSやSANの比率を高めて流動性の改良を行う試みがなされている。しかし、このような改良法ではUL94燃焼試験で滴下物(ドリップ)を生じやすくなり、良好な難燃性が得られない。そこで、他の物性をなるべく損なわず、難燃性をより改善する方法が強く望まれている。そしてそのような薄肉化指向から、厚さの薄いハウジング用途において、薄肉の(例えば3mm以下)、UL94の5V試験(5VB)に合格するような優れた難燃性を有する芳香族ポリカーボネート系の樹脂組成物が望まれている。
【0006】
そこで本発明は、UL94のV試験あるいは5V試験に代表される難燃性試験において優れた難燃性を有するポリカーボネート系の樹脂組成物を提供することを目的とする。
【0007】
【課題を解決するための手段】
本発明者らは、難燃剤と共に特定の2種類のゴムを組合せて、特定のポリカーボネート系の樹脂に添加すると、それぞれを単独で用いたときには予測できなかった程飛躍的に難燃性を改善できることを見出し、本発明に至った。
【0008】
本発明の難燃性樹脂組成物は、
(A)(A-1) 次式(化4):
【0009】
【化4】

Figure 0003675493
および次式(化5):
【0010】
【化5】
Figure 0003675493
(上記式中、R4 およびR5 はそれぞれ独立して、ハロゲン原子または一価の炭化水素基であり、Bは−(R1 −)C(−R2 )− [ここで、R1 およびR2 はそれぞれ独立して水素原子または1価の炭化水素基である]、−C(=R3 )− [ここでR3 は2価の炭化水素基である]、−O−、−S−、−SO−または−SO2 −であり、R6 は炭素数1〜10の炭化水素基もしくはそのハロゲン化物またはハロゲン原子であり、p、qおよびnはそれぞれ独立して0〜4の整数である)
で示される構造単位を有し、かつ前記(化5)の構造単位の量は(化4)および(化5)の構造単位の合計量の2〜90モル%を占めるところの共重合ポリカーボネートまたはこれとポリカーボネート系樹脂1〜100 重量部、ならびに(A-2) (a) 芳香族ビニル単量体成分および(b) シアン化ビニル単量体成分を、共重合体の構成成分として含む共重合体99〜0重量部を含み、かつ、(A)100重量部に対して、
(B)(a) 芳香族ビニル単量体成分、(b) シアン化ビニル単量体成分および(c) ゴム質重合体を、共重合体の構成成分として含む共重合体0.5 〜40重量部ならびに
(C)ポリオルガノシロキサンおよびポリアルキル(メタ)アクリレートを含む複合ゴムにビニル系単量体がグラフトしてなる複合ゴム系グラフト共重合体0.5 〜40重量部を含み、さらに(A)〜(C)の合計100重量部に対して、
(D)リン酸エステル系化合物1〜30重量部を含むことを特徴とする。
【0011】
本発明においては、成分(A)に、2種のゴム成分すなわち(B)と(C)および難燃剤(D)を組合せたところに特徴があり、(B)〜(D)のいずれか1つでも欠けると、良好な難燃性は得られない。
【0012】
本発明においては、成分(A)の(A-1) は、上記した共重合ポリカーボネートまたはこれとポリカーボネート系樹脂である。
【0013】
本発明で使用する共重合ポリカーボネートは、上記式(化4)および(化5)で示される構成単位を有することが必要である。まず、(化4)で示される構成単位はジフェノール成分およびカーボネート成分よりなる。ジフェノール成分を導入するために使用できるジフェノールを次式(化6)に示す。
【0014】
【化6】
Figure 0003675493
上記式中、R4 、R5 、B、pおよびqは、先に示したのと同義である。
【0015】
本発明において有効なジフェノールとしては、例えば、ビス(4-ヒドロキシフェニル)メタン、1,1-ビス(4-ヒドロキシフェニル)エタン、2,2-ビス(4-ヒドロキシフェニル)プロパン(いわゆるビスフェノールA)、2,2-ビス(4-ヒドロキシフェニル)ブタン、2,2-ビス(4-ヒドロキシフェニル)オクタン、ビス(4-ヒドロキシフェニル)フェニルメタン、2,2-ビス(4-ヒドロキシ-1- メチルフェニル)プロパン、1,1-ビス(4-ヒドロキシ-t- ブチルフェニル)プロパン、2,2-ビス(4-ヒドロキシ-3- ブロモフェニル)プロパンなどのビス(ヒドロキシアリール)アルカン類;1,1-ビス(4-ヒドロキシフェニル)シクロペンタン、1,1-ビス(4-ヒドロキシフェニル)シクロヘキサンなどのビス(ヒドロキシアリール)シクロアルカン類;4,4'- ジヒドロキシジフェニルエーテル、4,4'- ジヒドロキシ-3,3'-ジメチルフェニルエーテルなどのジヒドロキシアリールエーテル類;4,4'- ジヒドロキシジフェニルスルフィド、4,4'- ジヒドロキシ-3,3'-ジメチルジフェニルスルフィドなどのジヒドロキシジアリールスルフィド類;4,4'- ジヒドロキシジフェニルスルホキシド、4,4'- ジヒドロキシ-3,3'-ジメチルジフェニルスルホキシドなどのジヒドロキシジアリールスルホキシド類;4,4'- ジヒドロキシジフェニルスルホン、4,4'- ジヒドロキシ-3,3'-ジメチルジフェニルスルホンなどのジヒドロキシジアリールスルホン類などが挙げられるが、これらに限定されない。これらを1種または2種以上組合せて使用することができる。これらのうちでは、特に2,2-ビス(4-ヒドロキシフェニル)プロパンが好ましい。
【0016】
またカーボネート成分を導入するための前駆物質としては、例えばジフェニルカーボネート、ジトリールカーボネート、ビス(クロロフェニル)カーボネート、m-クレジルカーボネート、ジナフチルカーボネート、ビス(ジフェニル)カーボネート、ジエチルカーボネート、ジメチルカーボネート、ジブチルカーボネート、ジシクロヘキシルカーボネートなどの炭酸ジエステル、およびホスゲンなどのハロゲン化カルボニル化合物等が挙げられる。これらを1種または2種以上組合せて使用することができる。特にジフェニルカーボネートが好ましい。
【0017】
次に、上記式(化5)で示される構造単位は、ジフェノール成分、レゾルシンおよび/または置換レゾルシン成分ならびにカーボネート成分から成る。ジフェノール成分の導入については、上記したのと同様のジフェノールを使用できる。またカーボネート成分としては、上記した炭酸ジエステルまたはホスゲンを使用できる。レゾルシンおよび/または置換レゾルシン成分の導入のためには、次式(化7):
【0018】
【化7】
Figure 0003675493
(ここで、R6 およびnは上記と同義である)
で示される化合物を1種または2種以上組合せて使用することができる。このような化合物としては、例えばレゾルシン、および3-メチルレゾルシン、3-エチルレゾルシン、3-プロピルレゾルシン、3-ブチルレゾルシン、3-t-ブチルレゾルシン、3-フェニルレゾルシン、3-クミルレゾルシン、2,3,4,6-テトラフルオロレゾルシン、2,3,4,6-テトラブロモレゾルシンなどの置換レゾルシンが挙げられる。これらのうち特にレゾルシンが好ましい。
【0019】
共重合ポリカーボネートは、(化4)(化5)で示される上記した2種の構成単位を次の割合で有している。すなわち、(化5)で示される構成単位の量が、(化4)および(化5)の合計量の2〜90モル%、好ましくは2〜40モル%である。(化5)の量が2モル%より少ないとガラス転移温度(Tg)の低下が不十分であるので、流動性の改良効果がみられない。また、90モル%より多いと従来のポリカーボネートと同等の優れた物性、例えば機械的強度、耐熱性等が得られない。
【0020】
共重合ポリカーボネートの重量平均分子量は、通常10,000〜100,000 、好ましくは18,000〜40,000である。ここでいう重量平均分子量とは、ポリカーボネート用に補正されたポリスチレンを用いて、GPC(ゲル浸透クロマトグラフィー)によって測定されたものである。(また、メチレンクロリド中、25℃で測定した固有粘度が、0.35〜0.65 dl/g であるものが好ましい。)
共重合ポリカーボネートは、公知のポリカーボネートの製造方法、例えばホスゲンを用いる界面重合法、溶融重合法等によって製造できる。特に溶融重合法は毒性物質であるホスゲンや塩化メチレン等を用いないので、環境衛生上好ましい。
【0021】
溶融重合反応の際の温度、圧力等の条件は任意であり、公知の慣用の条件を用いることができる。具体的には、好ましくは80〜250 ℃、より好ましくは 100〜230 ℃、特に好ましくは 120〜190 ℃の温度で、好ましくは0〜5時間、より好ましくは0〜4時間、特に好ましくは0〜3時間、常圧下で、ジフェノールおよび上記式(化7)で示される化合物と炭酸ジエステルとを反応させる。次いで、反応系を減圧にしながら反応温度を高めて、ジフェノールおよび上記式(化7)で示される化合物と炭酸ジエステルとの反応を行い、最終的には5mmHg以下、より好ましくは1mmHg以下の減圧下で 240〜320 ℃の温度で、ジフェノールおよび上記式(化7)で示される化合物と、炭酸ジエステルとの反応を行うのが好ましい。
【0022】
上記のような重縮合反応は、連続式で行っても良く、バッチ式で行っても良い。また、上記反応を行う際に使用する反応装置は、槽型であっても、管型であっても、塔型であっても良い。
【0023】
またこの溶融重合法によれば、得られる共重合ポリカーボネートにおける構造単位(化5)が(化4)および(化5)の合計の90モル%を超えるような割合で、すなわちレゾルシンおよび/または置換レゾルシンを、ジフェノール100モルに対して、90モルを超えるような量で使用しても、他の方法、例えば界面重合法等に比べて、色相、耐水性、耐熱性の優れた共重合ポリカーボネートが得られる。
【0024】
また、共重合ポリカーボネートは、その末端がフェノールであっても十分な耐衝撃強度を有するが、p-t-ブチルフェノール、イソノニルフェノール、イソオクチルフェノール、m-またはp-クミルフェノール(好ましくはp-クミルフェノール)、クロマニル化合物、例えばクロマンのような、よりかさ高い末端基を導入すると、より低温衝撃性が優れた共重合ポリカーボネートを得ることができる。
【0025】
成分(A)は、上記の共重合ポリカーボネートと共に任意的に、ポリカーボネート系樹脂を含むことができる。本発明において使用されるポリカーボネート系樹脂は、公知のホスゲン法または溶融法により作られた芳香族ポリカーボネートである(例えば特開昭63-215763 号公報および特開平2-124934号公報参照)。
【0026】
成分(A)が共重合ポリカーボネートおよびポリカーボネート系樹脂の両方を含む場合には、両者の配合比率は任意である。
【0027】
また、(A-1) は、塩化メチレン中、25℃で測定した固有粘度が、0.32〜0.65 dl/g であるものが好ましい。
【0028】
次に、成分(A)は任意的に、(A-2) (a) 芳香族ビニル単量体成分および(b) シアン化ビニル単量体成分を含む共重合体を含有することができる。樹脂組成物の難燃性向上のためには(A-2) 成分は必須ではないが、(A-2) 成分を含有すると、成形性(流動性)が改善されるので好ましい。
【0029】
(a) 芳香族ビニル単量体成分としては、例えばスチレン、α‐メチルスチレン、o-,m- もしくはp-メチルスチレン、ビニルキシレン、モノクロロスチレン、ジクロロスチレン、モノブロモスチレン、ジブロモスチレン、フルオロスチレン、p-tert- ブチルスチレン、エチルスチレン、ビニルナフタレン等を挙げることができ、これらを1種または2種以上使用する。好ましくはスチレン、α‐メチルスチレンである。
【0030】
(b) シアン化ビニル単量体成分としては、例えばアクリロニトリル、メタクリロニトリル等を挙げることができ、これらを1種または2種以上使用する。これらの組成比は特に制限されず、用途に応じて選択される。
【0031】
(a)/(b) の組成比は特に限定されないが、(A-2) 成分中において好ましくは(a) が95〜50重量%、(b) が5〜50重量%であり、さらに好ましくは(a) が92〜65重量%、(b) が8〜35重量%である。
【0032】
(A-2) の共重合体の好ましい例としては、例えばSAN樹脂(スチレン‐アクリロニトリル共重合体)が挙げられる。
【0033】
(A-2) の共重合体の製造法に関しては特に制限はなく、塊状重合、溶液重合、塊状懸濁重合、懸濁重合、乳化重合など通常公知の方法が用いられる。また、別々に共重合した樹脂をブレンドすることによって得ることも可能である。
【0034】
成分(A)における(A-1) および(A-2) の配合比率は、(A-1) 1〜100重量部に対して(A-2) を99〜0重量部、好ましくは(A-1) 10〜99重量部に対して(A-2) を90〜1重量部である。
【0035】
次に成分(B)について述べる。(B)は(a) 芳香族ビニル単量体成分、(b) シアン化ビニル単量体成分および(c) ゴム質重合体を含む共重合体である。(a) 芳香族ビニル単量体成分および(b) シアン化ビニル単量体成分については、前記した成分(A)の(A-2) において示したものが挙げられる。(c) ゴム質重合体としては、ポリブタジエン、ポリイソプレン、スチレン‐ブタジエンのランダム共重合体およびブロック共重合体、該ブロック共重合体の水素添加物、アクリロニトリル‐ブタジエン共重合体、ブタジエン‐イソプレン共重合体などのジエン系ゴム、エチレン‐プロピレンのランダム共重合体およびブロック共重合体、エチレン‐ブテンのランダム共重合体およびブロック共重合体、エチレンとα‐オレフィンとの共重合体、エチレン‐メタクリレート、エチレン‐ブチルアクリレートなどのエチレン‐不飽和カルボン酸エステルとの共重合体、アクリル酸エステル‐ブタジエン共重合体、例えばブチルアクリレート‐ブタジエン共重合体などのアクリル系弾性重合体、エチレン‐酢酸ビニルなどのエチレンと脂肪酸ビニルとの共重合体、エチレン‐プロピレン‐エチリデンノルボルネン共重合体、エチレン‐プロピレン‐ヘキサジエン共重合体などのエチレン‐プロピレン非共役ジエンターポリマー、ブチレン‐イソプレン共重合体、塩素化ポリエチレンなどが挙げられ、これらを1種または2種以上で使用する。好ましいゴム質重合体としてはエチレン‐プロピレンゴム、エチレン‐プロピレン非共役ジエンターポリマー、ジエン系ゴムおよびアクリル系弾性重合体であり、特に好ましくはポリブタジエンおよびスチレン‐ブタジエン共重合体であり、このスチレン‐ブタジエン共重合体中のスチレン含有率は50重量%以下であることが好ましい。
【0036】
成分(B)において、各成分(a),(b) および(c) の組成比は特に制限はなく、用途に応じて各成分が配合される。
【0037】
成分(B)には、上記の成分(a),(b) および(c) の他に、(d) これらの成分と共重合可能な単量体を本発明の目的を損なわない範囲で使用することができる。そのような共重合可能な単量体としては、アクリル酸、メタクリル酸等のα,β‐不飽和カルボン酸、メチル(メタ)アクリレート、エチル(メタ)アクリレート、プロピル(メタ)アクリレート、ブチル(メタ)アクリレート、2-エチル (メタ)アクリレート、2-エチルヘキシルメタクリレート等のα,β‐不飽和カルボン酸エステル類;無水マレイン酸、無水イタコン酸等のα,β‐不飽和ジカルボン酸無水物類;マレイミド、N-メチルマレイミド、N-エチルマレイミド、N-フェニルマレイミド、N-o-クロロフェニルマレイミド等のα,β‐不飽和ジカルボン酸のイミド化合物類;等を挙げることができ、これらの単量体は1種または2種以上で使用される。
【0038】
成分(B)の共重合体としては、(c) ゴム質重合体の存在下にその他の成分がグラフト共重合したグラフト共重合体等が好ましく、さらに好ましくはABS樹脂(アクリロニトリル‐ブタジエン‐スチレン共重合体)、AES樹脂(アクリロニトリル‐エチレン‐プロピレン‐スチレン共重合体)、ACS樹脂(アクリロニトリル‐塩素化ポリエチレン‐スチレン共重合体)、AAS樹脂(アクリロニトリル‐アクリル系弾性重合体‐スチレン共重合体)である。
【0039】
成分(B)の共重合体の製造法については、上記の(A)の(A-2) の共重合体と同様の方法が使用できる。
【0040】
上記の成分(B)は、成分(A)100 重量部に対して0.5 〜40重量部、好ましくは0.5 〜30重量部添加する。成分(B)の量が上記の範囲より少ないと、本発明の効果が発揮されず、上記の範囲より多いと剛性が低下する。
【0041】
次に、本発明で使用する成分(C)は、ポリオルガノシロキサンゴム成分とポリアルキル(メタ)アクリレートゴム成分とが交互に絡み合って複合一体化されている構造を有する複合ゴムに、1種または2種以上のビニル系単量体がグラフト重合されてなる複合ゴム系グラフト共重合体である。
【0042】
このような複合ゴム系グラフト共重合体の製造は、例えば特開昭64-79257号公報明細書等に記載された方法を用いることができる。
【0043】
このような複合ゴムは、乳化重合法によって製造するのが適している。まずポリオルガノシロキサンゴムのラテックスを調製し、次にアルキル(メタ)アクリレートゴムの合成用単量体をポリオルガノシロキサンゴムラテックスのゴム粒子に含浸させてから、アルキル(メタ)アクリレートゴムの合成用単量体を重合させるのが好ましい。
【0044】
ポリオルガノシロキサンゴム成分は、例えば以下に示すオルガノシロキサンおよび架橋剤(I)を用いて乳化重合により調製することができ、その際、さらにグラフト交叉剤(I)を併用することができる。
【0045】
オルガノシロキサンとしては、例えば、ジメチルシロキサン等の鎖状オルガノシロキサンが挙げられる。また、3員環以上、好ましくは3〜6員環の各種の環状オルガノシロキサンを用いることもできる。例えばヘキサメチルシクロトリシロキサン、オクタメチルシクロテトラシロキサン、デカメチルシクロペンタシロキサン、ドデカメチルシクロヘキサシロキサン、トリメチルトリフェニルシクロトリシロキサン、テトラメチルテトラフェニルシクロテトラシロキサン、オクタフェニルシクロテトラシロキサン等が挙げられる。これらのオルガノシロキサンを単独でまたは2種以上混合して用いることができる。これらの使用量は、好ましくはポリオルガノシロキサンゴム成分中50重量%以上、さらに好ましくは70重量%以上である。
【0046】
架橋剤(I)としては、3官能性または4官能性のシラン系架橋剤、例えばトリメトキシメチルシラン、トリエトキシフェニルシラン、テトラメトキシシラン、テトラエトキシシラン、テトラ-n- プロポキシシラン、テトラブトキシシラン等を用いることができる。特に4官能性の架橋剤が好ましく、この中でもテトラエトキシシランが特に好ましい。架橋剤は単独で用いてもよく、また2種以上併用してもよい。架橋剤の使用量はポリオルガノシロキサンゴム成分中0.1〜30重量%が好ましい。
【0047】
グラフト交叉剤(I)としては、次式:
【0048】
【化8】
CH2 =C(R2 )−COO−(CH2 p −SiR1 n (3-n)/2 (I−1)
【0049】
【化9】
CH2 =CH−SiR1 n (3-n)/2 (I−2)
または
【0050】
【化10】
HS−(CH2 p −SiR1 n (3-n)/2 (I−3)
(上記式中、R1 は低級アルキル基、例えばメチル基、エチル基、プロピル基等またはフェニル基を表し、R2 は水素原子またはメチル基を表し、nは0、1または2を表し、pは1〜6の整数を表す)
で示される単位を形成し得る化合物が用いられる。上記式(I−1)の単位を形成し得る(メタ)アクリロイルオキシシロキサンはグラフト効率が高いため、有効なグラフト鎖を形成することが可能であり、高い耐衝撃性を発現するという点で有利である。なお、式(I−1)の単位を形成し得るものとしてメタクリロイルオキシシロキサンが特に好ましい。メタクリロイルオキシシロキサンの具体例としては、β‐メタクリロイルオキシエチルジメトキシメチルシラン、γ‐メタクリロイルオキシプロピルメトキシジメチルシラン、γ‐メタクリロイルオキシプロピルジメトキシメチルシラン、γ‐メタクリロイルオキシプロピルトリメトキシシラン、γ‐メタクリロイルオキシプロピルエトキシジエチルシラン、γ‐メタクリロイルオキシプロピルジエトキシメチルシラン、δ‐メタクリロイルオキシブチルジエトキシメチルシラン等が挙げられる。これらは単独で用いてもよく、また2種以上併用してもよい。グラフト交叉剤の使用量は、好ましくはポリオルガノシロキサンゴム成分中0〜10重量%である。
【0051】
このポリオルガノシロキサンゴム成分のラテックスの製造は、例えば米国特許第2891920 号明細書、同第3294725 号明細書等に記載された方法を用いることができる。本発明の実施では、例えばオルガノシロキサンと架橋剤(I)および所望によりグラフト交叉剤(I)の混合溶液とを、アルキルベンゼンスルホン酸、アルキルスルホン酸等のスルホン酸系乳化剤の存在下で、例えばホモジナイザー等を用いて水と剪断混合する方法により製造することが好ましい。アルキルベンゼンスルホン酸はオルガノシロキサンの乳化剤として作用すると同時に重合開始剤ともなるので好適である。この際、アルキルベンゼンスルホン酸の金属塩、アルキルスルホン酸の金属塩等を併用すると、グラフト重合を行う際にポリマーを安定に維持するのに効果があるので好ましい。
【0052】
次に、上記複合ゴムを構成するポリアルキル(メタ)アクリレートゴム成分は、以下に示すアルキル(メタ)アクリレート、架橋剤(II)およびグラフト交叉剤(II)を用いて合成することができる。
【0053】
アルキル(メタ)アクリレートとしては、例えばメチルアクリレート、エチルアクリレート、n-プロピルアクリレート、n-ブチルアクリレート、2-エチルヘキシルアクリレート等のアルキルアクリレートおよびヘキシルメタクリレート、2-エチルヘキシルメタクリレート、n-ラウリルメタクリレート等のアルキルメタクリレートが挙げられ、特にn-ブチルアクリレートの使用が好ましい。
【0054】
架橋剤(II)としては、例えばエチレングリコールジメタクリレート、プロピレングリコールジメタクリレート、1,3-ブチレングリコールジメタクリレート、1,4-ブチレングリコールジメタクリレート等が挙げられる。
【0055】
グラフト交叉剤(II)としては、例えばアリルメタクリレート、トリアリルシアヌレート、トリアリルイソシアヌレート等が挙げられる。アリルメタクリレートは架橋剤として用いることもできる。これら架橋剤およびグラフト交叉剤は単独で用いてもよく、また2種以上併用しても良い。これら架橋剤およびグラフト交叉剤の合計の使用量は、好ましくはポリアルキル(メタ)アクリレートゴム成分中0.1〜20重量%である。
【0056】
ポリアルキル(メタ)アクリレートゴム成分の重合は、水酸化ナトリウム、水酸化カリウム、炭酸ナトリウム等のアルカリの水溶液の添加により中和されたポリオルガノシロキサンゴム成分のラテックス中へ上記アルキル(メタ)アクリレート、架橋剤およびグラフト交叉剤を添加し、ポリオルガノシロキサンゴム粒子へ含浸させた後、通常のラジカル重合開始剤を作用させて行う。重合の進行と共にポリオルガノシロキサンゴムの架橋網目に相互に絡んだポリアルキル(メタ)アクリレートゴムの架橋網目が形成され、実質上分離できない、ポリオルガノシロキサンゴム成分とポリアルキル(メタ)アクリレートゴム成分との複合ゴムのラテックスが得られる。なお、本発明の実施に際しては、この複合ゴムとしてポリオルガノシロキサンゴム成分の主骨格がジメチルシロキサンの繰り返し単位を有し、ポリアルキル(メタ)アクリレートゴム成分の主骨格がn-ブチルアクリレートの繰り返し単位を有する複合ゴムが好ましく用いられる。
【0057】
この様にして乳化重合により調製された複合ゴムは、ビニル系単量体とグラフト共重合可能である。この複合ゴムをトルエンにより90℃で12時間抽出して測定したゲル含量は80重量%以上であると好ましい。
【0058】
また難燃性、耐衝撃性、外観等のバランスを満足させるためには、上記の複合ゴムにおけるポリオルガノシロキサンゴム成分とポリアルキル(メタ)アクリレートゴム成分の割合は、前者が3〜90重量%に対して後者が97〜10重量%であるのが好ましく、また、複合ゴムの平均粒子径は0.08〜0.6μmであるのが好ましい。
【0059】
上記の複合ゴムにグラフト重合させるビニル系単量体としては、スチレン、α‐メチルスチレン、ビニルトルエン等の芳香族アルケニル化合物;メチルメタクリレート、2-エチルヘキシルメタクリレート等のメタクリル酸エステル;メチルアクリレート、エチルアクリレート、ブチルアクリレート等のアクリル酸エステル;アクリロニトリル、メタクリロニトリル等のシアン化ビニル化合物等の各種ビニル系単量体が挙げられ、これらを単独でまたは2種以上組合せて用いることができる。特に好ましいビニル系単量体はメチルメタクリレートである。ビニル系単量体は、上記した複合ゴム30〜95重量%に対して5〜70重量%の割合で含まれると好ましい。
【0060】
複合ゴム系グラフト共重合体(C)は、上記ビニル系単量体を上記の複合ゴムのラテックスに加え、ラジカル重合技術によって一段または多段で重合させて得られる複合ゴム系グラフト共重合体ラテックスを、塩化カルシウムまたは硫酸マグネシウム等の金属塩を溶解した熱水中に投入し、塩析、凝固することにより分離、回収することができる。
【0061】
このような複合ゴム系グラフト共重合体(C)は、例えば三菱レイヨン株式会社より、メタブレンS−2001として商業的に入手可能である。
【0062】
成分(C)は、成分(A)100 重量部に対して0.5 〜40重量部、好ましくは0.5 〜 30 重量部使用する。上記の範囲より少ないと、本発明の効果が発揮されず、上記の範囲より多いと剛性が低下する。
【0063】
本発明で使用する成分(D)リン酸エステル系化合物としては、次式(化11):
【0064】
【化11】
Figure 0003675493
(ここで、R1 、R2 、R3 およびR4 は、それぞれ独立して、水素原子または有機基を表すが、R1 =R2 =R3 =R4 =Hの場合を除く。Xは2価以上の有機基を表し、pは0または1であり、qは1以上、例えば30以下の整数、rは0以上の整数を表す。)
で示されるリン酸エステル系化合物が挙げられる。しかし、これ等に限定されるものではない。
【0065】
上記式において、有機基とはたとえば、置換されていてもいなくてもよいアルキル基、シクロアルキル基、アリール基等が挙げられる。また、置換されている場合、置換基としては例えばアルキル基、アルコキシ基、アルキルチオ基、ハロゲン、アリール基、アリールオキシ基、アリールチオ基、ハロゲン化アリール基等が挙げられ、またこれ等の置換基を組合せた基(例えばアリールアルコキシアルキル基等)またはこれ等の置換基を酸素原子、イオウ原子、窒素原子等により結合して組合せた基(例えば、アリールスルホニルアリール基等)を置換基として用いてもよい。また、2価以上の有機基とは上記した有機基から、炭素原子に結合している水素原子の1個以上を除いてできる2価以上の基を意味する。例えばアルキレン基、および好ましくは(置換)フェニレン基、多核フェノール類例えばビスフェノール類から誘導されるものが挙げられ、2以上の遊離原子価の相対的位置は任意である。特に好ましいものとして、ヒドロキノン、レゾルシノール、ジフェニロールメタン、ジフェニロールジメチルメタン、ジヒドロキシジフェニル、 p,p′- ジヒドロキシジフェニルスルホン、ジヒドロキシナフタレン等が挙げられる。
【0066】
具体的なリン酸エステル系化合物の例としては、トリメチルホスフェート、トリエチルホスフェート、トリブチルホスフェート、トリオクチルホスフェート、トリブトキシエチルホスフェート、トリフェニルホスフェート、トリクレジルホスフェート、クレジルフェニルホスフェート、オクチルジフェニルホスフェート、ジイソプロピルフェニルホスフェート、トリス(クロロエチル)ホスフェート、トリス(ジクロロプロピル)ホスフェート、トリス(クロロプロピル)ホスフェート、ビス(2,3-ジブロモプロピル)-2,3- ジクロロプロピルホスフェート、トリス(2,3-ジブロモプロピル)ホスフェートおよびビス(クロロプロピル)モノオクチルホスフェート、R1 〜R4 がアルコキシ例えばメトキシ、エトキシおよびプロポキシ、または好ましくは(置換)フェノキシ例えばフェノキシ、メチル(置換)フェノキシであるところのビスフェノールAビスホスフェート、ヒドロキノンビスホスフェート、レゾルシンビスホスフェート、トリオキシベンゼントリホスフェート等のポリホスフェートが挙げられ、好ましくはトリフェニルホスフェートおよび各種ポリホスフェートである。
【0067】
上記の成分(D)は、成分(A)〜(C)の合計100 重量部に対して1〜30重量部、好ましくは3〜20重量部添加する。成分(D)の量が上記の範囲より少ないと本発明の効果が十分発揮されず、上記の範囲より多いと耐熱性が損なわれる。
【0068】
本発明の樹脂組成物にはさらに、滴下防止剤を含むことができる。そのような滴下防止剤として使用することができるフッ素化ポリオレフィンは、商業的にも入手できるし、あるいは公知の方法によって製造することもできる。それは、たとえば、遊離基触媒(たとえばペルオキシ二硫酸ナトリウム、カリウムまたはアンモニウム)を使用しながら水性媒質中において 100〜1000psi の圧力および0〜 200℃好ましくは20〜 100℃の温度下でテトラフルオロエチレンを重合させることによって得られる白色の固体である。詳しくは、ブルベーカー(Brubaker)の米国特許第 2,393,967号明細書を参照されたい。不可欠ではないが、比較的大きな粒子たとえば平均粒度 0.3〜 0.7mm(主として 0.5mm)の粒子の状態にある樹脂を使用することが好ましい。これは0.05〜 0.5mmの粒度を有する通常のポリテトラフルオロエチレン粉末よりも良好である。かかる比較的大きな粒度の物質が特に好ましい理由は、それが重合体中に容易に分散しかつ重合体同志を結合して繊維状材料を作る傾向を示すことにある。かかる好適なポリテトラフルオロエチレンはASTMによればタイプ3と呼ばれるもので、実際にはデュポン社(E.I.Dupont de Nemours and Company )からテフロン6(Teflon 6)として商業的に入手し得る。あるいは、三井デュポンフロロケミカル社のテフロン30Jとして商業的に入手し得る。フッ素化ポリオレフィンは、成分(A)100 重量部に対して、好ましくは0.01〜2重量部、より好ましくは0.05〜1.0 重量部使用する。
【0069】
本発明の樹脂組成物には、上記の成分の他に、その物性を損なわない限りにおいて、その目的に応じて樹脂の混合時、成形時に、慣用の他の添加剤、例えば顔料、染料、補強剤(ガラス繊維、炭素繊維など)、充填剤(カーボンブラック、シリカ、酸化チタンなど)、耐熱剤、酸化劣化防止剤、耐候剤、滑剤、離型剤、結晶核剤、可塑剤、流動性改良剤、帯電防止剤等を添加することができる。
【0070】
本発明の樹脂組成物を製造するための方法に特に制限はなく、通常の方法が満足に使用できる。しかしながら一般に溶融混合法が望ましい。少量の溶剤の使用も可能であるが、一般に必要ない。装置としては特に押出機、バンバリーミキサー、ローラー、ニーダー等を例として挙げることができ、これらを回分的または連続的に運転する。成分の混合順は特に限定されない。
【0071】
【実施例】
以下の実施例により、本発明をさらに詳しく説明する。なお、実施例においては以下の成分を使用した。
成分 (A-1)
RS−PC:以下のようにして製造した共重合ポリカーボネート;
ビスフェノールA(日本ジーイープラスチックス株式会社製)0.22キロモル、レゾルシン0.22キロモルおよびジフェニルカーボネート(エニィ社製)0.44キロモルを、第1の槽型撹拌機(容量250リットル)に仕込み、140℃で溶融した。この温度に保持しながら、得られた混合物を、ビスフェノールA換算で毎時0.16キロモルの速度で、第2の槽型撹拌機(容量50リットル)に送液した。第2の槽型撹拌機の温度は180℃に保持した。
【0072】
ここに触媒として、テトラメチルアンモニウムヒドロキシドを毎時0.04モルおよび水酸化ナトリウムを毎時0.00016モル(1×10-6モル/モル‐ビスフェノールA)添加し、滞留時間が30分間となるように時間を調整し、撹拌した。
【0073】
次に、この反応液を、ビスフェノールA換算で毎時0.16キロモルの速度で、第3の槽型撹拌機(容量50リットル)に送液した。第3の槽型撹拌機の温度は210℃、圧力は200mmHgであった。滞留時間が30分間となるように時間を調整し、フェノールを抽出除去しながら撹拌した。
【0074】
次に、この反応液を、ビスフェノールA換算で毎時0.16キロモルの速度で、第4の槽型撹拌機(容量50リットル)に送液した。第4の槽型撹拌機の温度は240℃、圧力は15mmHgであった。滞留時間が30分間となるように時間を調整し、フェノールを抽出除去しながら撹拌した。反応が定常になって得られた反応物の極限粘度[η]は0.15dl/gであった。
【0075】
次に、この反応物をギアポンプで昇圧し、ビスフェノールA換算で毎時0.16キロモルの速度で、遠心式薄膜蒸発機に送入し、反応を進めた。薄膜蒸発機の温度および圧力はそれぞれ、270℃および2mmHgに制御した。反応物を、蒸発機下部よりギアポンプにて、290℃および0.2mmHgに制御された二軸横型撹拌重合槽(L/D=3、撹拌翼回転直径 220mm、内容積80リットル)に、ビスフェノールA換算で毎時0.16キロモルの速度(約40kg/ 時間)で送り込み、滞留時間30分間にて重合させた。このときの生成物の極限粘度[η]は0.49dl/gであった。生成物は、次式(化12)および(化13)をモル比50:50で有する共重合ポリカーボネートであった。以下ではこれをRS−PCと略記する。
【0076】
【化12】
Figure 0003675493
【0077】
【化13】
Figure 0003675493
PC(1):ビスフェノールAのポリカーボネート(商標;レキサン、日本ジーイープラスチックス株式会社製)、塩化メチレン中、25℃で測定した固有粘度0.56dl/g
PC(2):ビスフェノールAのポリカーボネート(商標;レキサン、日本ジーイープラスチックス株式会社製)、塩化メチレン中、25℃で測定した固有粘度0.50dl/g
PC(3):ビスフェノールAのポリカーボネート(商標;レキサン、日本ジーイープラスチックス株式会社製)、塩化メチレン中、25℃で測定した固有粘度0.44dl/g
成分 (A-2)
SAN樹脂:商標SR 30B(ウベサイコン株式会社製)
成分(B)
ABS樹脂:商標UX 050(ウベサイコン株式会社製)
成分(C)
メタブレン S−2001:商標、メチルメタクリレート‐ブチルアクリレート‐ジメチルシロキサンコポリマー、三菱レイヨン株式会社製
成分(D)
CR733S:商標、フェニルレゾルシンポリホスフェート、大八化学株式会社製
任意成分
テフロン30J :商標、ポリテトラフルオロエチレン、三井デュポンフロロケミカル社製
実施例1および比較例1〜4
各成分を表1に示す割合(重量比)で混合し、240 ℃、150rpm に設定した2軸押出機(30mm)で押出し、ペレットを作成した。次いで、このペレットを、設定温度250 ℃、金型温度60℃で射出成形した。得られた成形品についてアイゾット衝撃強度およびメルトインデックス(MI)を測定し、難燃性の評価を行った。結果を表1に示す。
【0078】
なお、樹脂組成物の評価試験は、以下のようにして行った。
(1) アイゾット衝撃強度(Kg-cm/cm)
ASTM D 256に従って、厚み 1/8 インチ、ノッチ付で測定した。
(2) メルトインデックス(MI)
ASTM D 1238 に従って、温度260℃、5kg荷重の条件で測定した。
(3) 難燃性試験
UL94/V0,VI,VII試験
5個の試験棒をアンダーライターズラボラトリーズインコーポレーションのブレチン94”材料分類のための燃焼試験”(以下、UL−94という)に示される試験方法にしたがって、厚み1/16インチで試験した。この試験方法により、供試材料を、5個の試料の結果に基づいてUL−94 V−0、V−IおよびV−IIのいずれかの等級に評価した。UL−94についての各Vの等級の基準は概略次の通りである。
V−0:点火炎を取り除いた後の平均火炎保持時間が5秒以下であり、かつ全試料とも脱脂綿に着火する微粒炎を落下しない。
V−I:点火炎を取り除いた後の平均火炎保持時間が25秒以下であり、かつ全試料とも脱脂綿に着火する微粒炎を落下しない。
V−II:点火炎を取り除いた後の平均火炎保持時間が25秒以下であり、かつこれらの試料が脱脂綿に着火する微粒炎を落下する。
【0079】
また、UL−94は全試験棒が特定のV等級に合格しなければ、その等級に分類してはならない旨を規定している。この条件を満たさない場合には、その5個の試験棒は最も成績の悪い1個の試験棒の等級を与えられる。例えば1個の試験棒がV−IIに分類された場合には、5個の全試験棒に対する等級はV−IIである。
UL94/5V(5VB)試験(5インチフラムテスト)
A法(バー試験)により、試験片をバーナに5回あてて、(1) 燃焼時間とグローイングの時間、(2) 試験片の燃えた距離、(3) 滴下物(ドリップ)の有無、(4)変形と物理的強度の観察を行った。なお、試験片の厚みは2.5mmであった。5VB合格判定基準:どの試験片も試験炎を5回あてた後の燃焼時間および、またはグローイングは60秒を超えない。かつどの試験片も滴下物がない。
【0080】
【表1】
Figure 0003675493
【0081】
【発明の効果】
本発明により、薄く成形されても難燃性が著しく優れたポリカーボネート系樹脂組成物を提供することができる。本発明の樹脂組成物は特に、滴下物抑制効果が高い。よって、本発明の樹脂組成物は、工業的に非常に有用である。[0001]
[Industrial application fields]
The present invention relates to a flame retardant resin composition containing a polycarbonate-based resin.
[0002]
[Background Art and Problems to be Solved by the Invention]
Polycarbonate resins are used in various applications because of their excellent heat resistance, impact resistance, etc., but have disadvantages such as high molding temperature, poor flowability, and large thickness dependence of impact strength. doing.
[0003]
Therefore, attempts have been made to solve these problems by blending polycarbonate (PC) resin with ABS (acrylonitrile-butadiene-styrene) resin (Japanese Patent Publication No. 38-15225, Japanese Patent Publication No. 48-12170). No., JP-B 57-21530, JP-B 58-46269, etc.).
[0004]
By the way, PC / ABS alloy is excellent in moldability and impact resistance, but since flame retardance is insufficient, various attempts have been made to improve flame retardancy (Japanese Patent Publication No. Sho 54-30417). JP, 61-62556, A).
[0005]
However, in recent years, with the demand for cost reduction and weight reduction of devices, the trend toward thinning is increasing. In order to achieve thinning of the material, for example, attempts have been made to improve flowability by, for example, reducing the molecular weight of polycarbonate or increasing the ratio of ABS or SAN. However, with such an improved method, dripping is likely to occur in the UL94 combustion test, and good flame retardancy cannot be obtained. Therefore, there is a strong demand for a method for further improving flame retardancy without impairing other physical properties as much as possible. From such a thin-walled orientation, an aromatic polycarbonate resin having excellent flame retardancy that passes the UL94 5V test (5 VB) for thin housing applications (eg, 3 mm or less). A composition is desired.
[0006]
Accordingly, an object of the present invention is to provide a polycarbonate-based resin composition having excellent flame retardancy in a flame retardancy test represented by a UL94 V test or a 5V test.
[0007]
[Means for Solving the Problems]
When the present inventors combine two specific types of rubber together with a flame retardant and add them to a specific polycarbonate-based resin, the flame retardancy can be drastically improved when they are not expected when used alone. And found the present invention.
[0008]
The flame retardant resin composition of the present invention is
(A) (A-1) The following formula (Formula 4):
[0009]
[Formula 4]
Figure 0003675493
And the following formula (Formula 5):
[0010]
[Chemical formula 5]
Figure 0003675493
(In the above formula, RFourAnd RFiveEach independently represents a halogen atom or a monovalent hydrocarbon group, and B represents — (R1-) C (-R2)-[Where R1And R2Are each independently a hydrogen atom or a monovalent hydrocarbon group], -C (= RThree)-[Where RThreeIs a divalent hydrocarbon group], -O-, -S-, -SO- or -SO2-And R6Is a hydrocarbon group having 1 to 10 carbon atoms, a halide thereof, or a halogen atom, and p, q and n are each independently an integer of 0 to 4)
And the amount of the structural unit of (Chemical Formula 5) occupies 2 to 90 mol% of the total amount of the structural units of (Chemical Formula 4) and (Chemical Formula 5) or A copolymer containing 1 to 100 parts by weight of this and a polycarbonate-based resin, and (A-2) (a) an aromatic vinyl monomer component and (b) a vinyl cyanide monomer component as components of the copolymer. Including 99 to 0 parts by weight of coalescence, and (A) 100 parts by weight,
(B) (a) aromatic vinyl monomer component, (b) vinyl cyanide monomer component, and (c) a copolymer containing 0.5 to 40 parts by weight of a rubbery polymer as a constituent of the copolymer And
(C) 0.5 to 40 parts by weight of a composite rubber-based graft copolymer obtained by grafting a vinyl-based monomer onto a composite rubber containing polyorganosiloxane and polyalkyl (meth) acrylate, and (A) to (C ) For a total of 100 parts by weight
(D) It contains 1 to 30 parts by weight of a phosphoric ester compound.
[0011]
In the present invention, the component (A) is characterized by combining two rubber components, that is, (B) and (C) and the flame retardant (D), and any one of (B) to (D) If one is missing, good flame retardancy cannot be obtained.
[0012]
In the present invention, the component (A) (A-1) is the above-mentioned copolymer polycarbonate or this and a polycarbonate resin.
[0013]
The copolymeric polycarbonate used in the present invention needs to have structural units represented by the above formulas (Chemical Formula 4) and (Chemical Formula 5). First, the structural unit represented by (Chemical Formula 4) comprises a diphenol component and a carbonate component. The diphenol that can be used to introduce the diphenol component is shown in the following formula (Formula 6).
[0014]
[Chemical 6]
Figure 0003675493
In the above formula, RFour, RFive, B, p and q are as defined above.
[0015]
Examples of diphenols effective in the present invention include bis (4-hydroxyphenyl) methane, 1,1-bis (4-hydroxyphenyl) ethane, and 2,2-bis (4-hydroxyphenyl) propane (so-called bisphenol A). ), 2,2-bis (4-hydroxyphenyl) butane, 2,2-bis (4-hydroxyphenyl) octane, bis (4-hydroxyphenyl) phenylmethane, 2,2-bis (4-hydroxy-1-) Bis (hydroxyaryl) alkanes such as methylphenyl) propane, 1,1-bis (4-hydroxy-t-butylphenyl) propane, 2,2-bis (4-hydroxy-3-bromophenyl) propane; Bis (hydroxyaryl) cycloalkanes such as 1-bis (4-hydroxyphenyl) cyclopentane and 1,1-bis (4-hydroxyphenyl) cyclohexane; 4,4'-dihydroxydiphenyl Ethers, dihydroxyaryl ethers such as 4,4'-dihydroxy-3,3'-dimethylphenyl ether; 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfide, etc. Dihydroxydiaryl sulfides; 4,4'-dihydroxydiphenyl sulfoxide, dihydroxydiaryl sulfoxides such as 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide; 4,4'-dihydroxydiphenyl sulfone, 4,4'- Examples thereof include, but are not limited to, dihydroxydiaryl sulfones such as dihydroxy-3,3′-dimethyldiphenyl sulfone. These can be used alone or in combination of two or more. Of these, 2,2-bis (4-hydroxyphenyl) propane is particularly preferable.
[0016]
Examples of the precursor for introducing the carbonate component include diphenyl carbonate, ditolyl carbonate, bis (chlorophenyl) carbonate, m-cresyl carbonate, dinaphthyl carbonate, bis (diphenyl) carbonate, diethyl carbonate, dimethyl carbonate, and dibutyl. Examples thereof include carbonic acid diesters such as carbonate and dicyclohexyl carbonate, and halogenated carbonyl compounds such as phosgene. These can be used alone or in combination of two or more. Diphenyl carbonate is particularly preferable.
[0017]
Next, the structural unit represented by the above formula (Formula 5) comprises a diphenol component, a resorcin and / or substituted resorcin component, and a carbonate component. For the introduction of the diphenol component, the same diphenol as described above can be used. As the carbonate component, the above-mentioned carbonic acid diester or phosgene can be used. For the introduction of resorcin and / or substituted resorcin components, the following formula:
[0018]
[Chemical 7]
Figure 0003675493
(Where R6And n are as defined above)
These compounds can be used singly or in combination of two or more. Examples of such compounds include resorcin, 3-methylresorcin, 3-ethylresorcin, 3-propylresorcin, 3-butylresorcin, 3-t-butylresorcin, 3-phenylresorcin, 3-cumylresorcin, 2 , 3,4,6-tetrafluororesorcin, substituted resorcin such as 2,3,4,6-tetrabromoresorcin. Of these, resorcin is particularly preferred.
[0019]
The copolymer polycarbonate has the above-described two types of structural units represented by (Chemical Formula 4) and (Chemical Formula 5) in the following proportions. That is, the amount of the structural unit represented by (Chemical Formula 5) is 2 to 90 mol%, preferably 2 to 40 mol% of the total amount of (Chemical Formula 4) and (Chemical Formula 5). When the amount of (Chemical Formula 5) is less than 2 mol%, the glass transition temperature (Tg) is not sufficiently lowered, and thus the fluidity improving effect is not observed. On the other hand, if it exceeds 90 mol%, excellent physical properties equivalent to those of conventional polycarbonates, such as mechanical strength and heat resistance, cannot be obtained.
[0020]
The weight average molecular weight of the copolymerized polycarbonate is usually 10,000 to 100,000, preferably 18,000 to 40,000. The weight average molecular weight here is measured by GPC (gel permeation chromatography) using polystyrene corrected for polycarbonate. (It is also preferable that the intrinsic viscosity measured at 25 ° C. in methylene chloride is 0.35 to 0.65 dl / g.)
The copolymer polycarbonate can be produced by a known polycarbonate production method, for example, an interfacial polymerization method using phosgene, a melt polymerization method, or the like. In particular, the melt polymerization method does not use phosgene, methylene chloride, or the like which is a toxic substance, and thus is preferable in terms of environmental health.
[0021]
Conditions such as temperature and pressure during the melt polymerization reaction are arbitrary, and known conventional conditions can be used. Specifically, the temperature is preferably 80 to 250 ° C, more preferably 100 to 230 ° C, particularly preferably 120 to 190 ° C, preferably 0 to 5 hours, more preferably 0 to 4 hours, and particularly preferably 0. Diphenol and the compound represented by the above formula (Chemical Formula 7) are reacted with a carbonic acid diester under normal pressure for -3 hours. Next, the reaction temperature is raised while reducing the reaction system, and the reaction between diphenol and the compound represented by the above formula (Chemical Formula 7) and carbonic acid diester is carried out, and finally the reduced pressure is 5 mmHg or less, more preferably 1 mmHg or less It is preferable to carry out the reaction of diphenol and the compound represented by the above formula (Chemical Formula 7) with a carbonic acid diester at a temperature of 240 to 320 ° C.
[0022]
The polycondensation reaction as described above may be performed continuously or batchwise. Moreover, the reaction apparatus used when performing the said reaction may be a tank type, a tube type, or a tower type.
[0023]
Further, according to this melt polymerization method, the proportion of the structural unit (Chemical Formula 5) in the resulting copolymeric polycarbonate exceeds 90 mol% of the total of (Chemical Formula 4) and (Chemical Formula 5), that is, resorcin and / or substitution. Even if resorcin is used in an amount exceeding 90 moles relative to 100 moles of diphenol, it is a copolymer polycarbonate excellent in hue, water resistance and heat resistance compared to other methods such as interfacial polymerization. Is obtained.
[0024]
Copolycarbonate has sufficient impact strength even if the terminal is phenol, but pt-butylphenol, isononylphenol, isooctylphenol, m- or p-cumylphenol (preferably p-cumylphenol). ), Introducing a bulky end group such as a chromanyl compound, for example, chroman, can give a copolycarbonate having better low-temperature impact properties.
[0025]
The component (A) can optionally contain a polycarbonate-based resin together with the copolymer polycarbonate. The polycarbonate resin used in the present invention is an aromatic polycarbonate produced by a known phosgene method or melting method (see, for example, JP-A-63-215763 and JP-A-2-124934).
[0026]
When component (A) contains both a copolymer polycarbonate and a polycarbonate resin, the blending ratio of both is arbitrary.
[0027]
(A-1) preferably has an intrinsic viscosity measured at 25 ° C. in methylene chloride of 0.32 to 0.65 dl / g.
[0028]
Next, component (A) can optionally contain a copolymer comprising (A-2) (a) an aromatic vinyl monomer component and (b) a vinyl cyanide monomer component. The component (A-2) is not essential for improving the flame retardancy of the resin composition, but it is preferable to contain the component (A-2) because the moldability (fluidity) is improved.
[0029]
(a) Examples of aromatic vinyl monomer components include styrene, α-methylstyrene, o-, m- or p-methylstyrene, vinyl xylene, monochlorostyrene, dichlorostyrene, monobromostyrene, dibromostyrene, and fluorostyrene. , P-tert-butylstyrene, ethylstyrene, vinylnaphthalene and the like, and one or more of these are used. Styrene and α-methylstyrene are preferred.
[0030]
Examples of the (b) vinyl cyanide monomer component include acrylonitrile, methacrylonitrile and the like, and one or more of these are used. These composition ratios are not particularly limited, and are selected according to the application.
[0031]
The composition ratio of (a) / (b) is not particularly limited, but in the component (A-2), preferably (a) is 95 to 50% by weight, (b) is 5 to 50% by weight, and more preferably (A) is 92 to 65% by weight, and (b) is 8 to 35% by weight.
[0032]
Preferable examples of the copolymer (A-2) include a SAN resin (styrene-acrylonitrile copolymer).
[0033]
The method for producing the copolymer (A-2) is not particularly limited, and generally known methods such as bulk polymerization, solution polymerization, bulk suspension polymerization, suspension polymerization, and emulsion polymerization are used. It can also be obtained by blending separately copolymerized resins.
[0034]
The blending ratio of (A-1) and (A-2) in component (A) is 99 to 0 parts by weight of (A-2) to 1 to 100 parts by weight of (A-1), preferably (A -1) 90 to 1 part by weight of (A-2) with respect to 10 to 99 parts by weight.
[0035]
Next, the component (B) will be described. (B) is a copolymer comprising (a) an aromatic vinyl monomer component, (b) a vinyl cyanide monomer component, and (c) a rubbery polymer. Examples of the (a) aromatic vinyl monomer component and the (b) vinyl cyanide monomer component include those shown in (A-2) of the aforementioned component (A). (c) Rubber polymers include polybutadiene, polyisoprene, random copolymers and block copolymers of styrene-butadiene, hydrogenated products of the block copolymers, acrylonitrile-butadiene copolymers, butadiene-isoprene copolymers. Diene rubbers such as polymers, ethylene-propylene random copolymers and block copolymers, ethylene-butene random copolymers and block copolymers, ethylene and α-olefin copolymers, ethylene-methacrylate , Copolymers with ethylene-unsaturated carboxylic esters such as ethylene-butyl acrylate, acrylic ester-butadiene copolymers, acrylic elastic polymers such as butyl acrylate-butadiene copolymers, ethylene-vinyl acetate, etc. Of ethylene and fatty acid vinyl Copolymer, ethylene-propylene-ethylidene norbornene copolymer, ethylene-propylene non-conjugated diene terpolymer such as ethylene-propylene-hexadiene copolymer, butylene-isoprene copolymer, chlorinated polyethylene, etc. Use by 1 type or 2 types or more. Preferred rubbery polymers are ethylene-propylene rubber, ethylene-propylene non-conjugated diene terpolymer, diene rubber and acrylic elastic polymer, particularly preferably polybutadiene and styrene-butadiene copolymer. The styrene content in the butadiene copolymer is preferably 50% by weight or less.
[0036]
In the component (B), the composition ratio of the components (a), (b) and (c) is not particularly limited, and each component is blended depending on the application.
[0037]
For component (B), in addition to the components (a), (b) and (c) above, (d) a monomer copolymerizable with these components is used within a range not impairing the object of the present invention. can do. Examples of such copolymerizable monomers include α, β-unsaturated carboxylic acids such as acrylic acid and methacrylic acid, methyl (meth) acrylate, ethyl (meth) acrylate, propyl (meth) acrylate, butyl (meta ) Α, β-unsaturated carboxylic esters such as acrylate, 2-ethyl (meth) acrylate, 2-ethylhexyl methacrylate; α, β-unsaturated dicarboxylic anhydrides such as maleic anhydride and itaconic anhydride; maleimide , N-methylmaleimides, N-ethylmaleimides, N-phenylmaleimides, No-chlorophenylmaleimides and the like, imide compounds of α, β-unsaturated dicarboxylic acids; Or it is used by 2 or more types.
[0038]
As the copolymer of component (B), (c) a graft copolymer in which other components are graft copolymerized in the presence of a rubbery polymer, and the like are preferable, and ABS resin (acrylonitrile-butadiene-styrene copolymer) is more preferable. Polymer), AES resin (acrylonitrile-ethylene-propylene-styrene copolymer), ACS resin (acrylonitrile-chlorinated polyethylene-styrene copolymer), AAS resin (acrylonitrile-acrylic elastic polymer-styrene copolymer) It is.
[0039]
Regarding the production method of the copolymer of component (B), the same method as the copolymer of (A-2) in (A) above can be used.
[0040]
The component (B) is added in an amount of 0.5 to 40 parts by weight, preferably 0.5 to 30 parts by weight, based on 100 parts by weight of the component (A). When the amount of the component (B) is less than the above range, the effect of the present invention is not exhibited, and when it is more than the above range, the rigidity is lowered.
[0041]
Next, the component (C) used in the present invention is a composite rubber having a structure in which a polyorganosiloxane rubber component and a polyalkyl (meth) acrylate rubber component are alternately entangled and combined into one or more types. A composite rubber-based graft copolymer obtained by graft polymerization of two or more vinyl monomers.
[0042]
For production of such a composite rubber-based graft copolymer, for example, a method described in JP-A No. 64-79257 can be used.
[0043]
Such a composite rubber is suitable to be produced by an emulsion polymerization method. First, a latex of polyorganosiloxane rubber is prepared, and then a monomer for synthesizing alkyl (meth) acrylate rubber is impregnated into the rubber particles of polyorganosiloxane rubber latex, followed by synthesis of alkyl (meth) acrylate rubber. It is preferred to polymerize the monomer.
[0044]
The polyorganosiloxane rubber component can be prepared by emulsion polymerization using, for example, the following organosiloxane and crosslinking agent (I), and in this case, the graft crossing agent (I) can be used in combination.
[0045]
Examples of the organosiloxane include chain organosiloxanes such as dimethylsiloxane. Also, various cyclic organosiloxanes having 3 or more members, preferably 3 to 6 members can be used. Examples thereof include hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, trimethyltriphenylcyclotrisiloxane, tetramethyltetraphenylcyclotetrasiloxane, octaphenylcyclotetrasiloxane, and the like. These organosiloxanes can be used alone or in admixture of two or more. The amount used thereof is preferably 50% by weight or more, more preferably 70% by weight or more in the polyorganosiloxane rubber component.
[0046]
As the crosslinking agent (I), trifunctional or tetrafunctional silane-based crosslinking agents such as trimethoxymethylsilane, triethoxyphenylsilane, tetramethoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetrabutoxysilane Etc. can be used. In particular, tetrafunctional crosslinking agents are preferred, and tetraethoxysilane is particularly preferred among these. A crosslinking agent may be used independently and may be used together 2 or more types. The amount of the crosslinking agent used is preferably 0.1 to 30% by weight in the polyorganosiloxane rubber component.
[0047]
As the graft crossing agent (I), the following formula:
[0048]
[Chemical 8]
CH2= C (R2) -COO- (CH2)p-SiR1 nO(3-n) / 2(I-1)
[0049]
[Chemical 9]
CH2= CH-SiR1 nO(3-n) / 2                (I-2)
Or
[0050]
[Chemical Formula 10]
HS- (CH2)p-SiR1 nO(3-n) / 2          (I-3)
(In the above formula, R1Represents a lower alkyl group such as a methyl group, an ethyl group, a propyl group or the like, or a phenyl group;2Represents a hydrogen atom or a methyl group, n represents 0, 1 or 2, and p represents an integer of 1 to 6)
The compound which can form the unit shown by is used. The (meth) acryloyloxysiloxane capable of forming the unit of the formula (I-1) has a high grafting efficiency, so that it can form an effective graft chain and is advantageous in that high impact resistance is expressed. It is. In addition, methacryloyloxysiloxane is particularly preferable as the unit capable of forming the unit of the formula (I-1). Specific examples of methacryloyloxysiloxane include β-methacryloyloxyethyldimethoxymethylsilane, γ-methacryloyloxypropylmethoxydimethylsilane, γ-methacryloyloxypropyldimethoxymethylsilane, γ-methacryloyloxypropyltrimethoxysilane, and γ-methacryloyloxypropyl. Examples include ethoxydiethylsilane, γ-methacryloyloxypropyldiethoxymethylsilane, and δ-methacryloyloxybutyldiethoxymethylsilane. These may be used alone or in combination of two or more. The amount of the grafting agent used is preferably 0 to 10% by weight in the polyorganosiloxane rubber component.
[0051]
For the production of the latex of the polyorganosiloxane rubber component, for example, a method described in US Pat. Nos. 2,891,920 and 3,32,725 can be used. In the practice of the present invention, for example, a mixed solution of an organosiloxane and a crosslinking agent (I) and optionally a graft crossing agent (I) is mixed with, for example, a homogenizer in the presence of a sulfonic acid-based emulsifier such as alkylbenzenesulfonic acid or alkylsulfonic acid. It is preferable to manufacture by the method of carrying out shear mixing with water using etc. Alkylbenzenesulfonic acid is suitable because it acts as an emulsifier for organosiloxane and at the same time serves as a polymerization initiator. In this case, it is preferable to use a metal salt of an alkylbenzene sulfonic acid, a metal salt of an alkyl sulfonic acid, or the like because it has an effect of maintaining a stable polymer during graft polymerization.
[0052]
Next, the polyalkyl (meth) acrylate rubber component constituting the composite rubber can be synthesized using the following alkyl (meth) acrylate, cross-linking agent (II) and graft crossing agent (II).
[0053]
Examples of the alkyl (meth) acrylate include alkyl acrylates such as methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, and 2-ethylhexyl acrylate, and alkyl methacrylates such as hexyl methacrylate, 2-ethylhexyl methacrylate, and n-lauryl methacrylate. In particular, the use of n-butyl acrylate is preferable.
[0054]
Examples of the crosslinking agent (II) include ethylene glycol dimethacrylate, propylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, 1,4-butylene glycol dimethacrylate and the like.
[0055]
Examples of the graft crossing agent (II) include allyl methacrylate, triallyl cyanurate, triallyl isocyanurate and the like. Allyl methacrylate can also be used as a crosslinking agent. These cross-linking agents and graft crossing agents may be used alone or in combination of two or more. The total amount of these crosslinking agents and grafting agents is preferably 0.1 to 20% by weight in the polyalkyl (meth) acrylate rubber component.
[0056]
The polymerization of the polyalkyl (meth) acrylate rubber component is carried out by adding the above alkyl (meth) acrylate into the latex of the polyorganosiloxane rubber component neutralized by the addition of an aqueous alkali solution such as sodium hydroxide, potassium hydroxide or sodium carbonate. After adding a cross-linking agent and a graft crossing agent and impregnating the polyorganosiloxane rubber particles, a normal radical polymerization initiator is allowed to act. A polyorganosiloxane rubber component and a polyalkyl (meth) acrylate rubber component, which form a crosslinked network of polyalkyl (meth) acrylate rubbers which are entangled with each other as the polymerization progresses, and are substantially inseparable. A composite rubber latex is obtained. In carrying out the present invention, as the composite rubber, the main skeleton of the polyorganosiloxane rubber component has a repeating unit of dimethylsiloxane, and the main skeleton of the polyalkyl (meth) acrylate rubber component is a repeating unit of n-butyl acrylate. A composite rubber having the following is preferably used.
[0057]
The composite rubber prepared by emulsion polymerization in this way can be graft copolymerized with a vinyl monomer. The gel content measured by extracting this composite rubber with toluene at 90 ° C. for 12 hours is preferably 80% by weight or more.
[0058]
In order to satisfy the balance of flame retardancy, impact resistance, appearance, etc., the ratio of the polyorganosiloxane rubber component to the polyalkyl (meth) acrylate rubber component in the above composite rubber is 3 to 90% by weight in the former. The latter is preferably 97 to 10% by weight, and the average particle size of the composite rubber is preferably 0.08 to 0.6 μm.
[0059]
Examples of vinyl monomers to be graft-polymerized on the above composite rubber include aromatic alkenyl compounds such as styrene, α-methylstyrene and vinyltoluene; methacrylic esters such as methyl methacrylate and 2-ethylhexyl methacrylate; methyl acrylate and ethyl acrylate And various vinyl monomers such as acrylic acid esters such as butyl acrylate; vinyl cyanide compounds such as acrylonitrile and methacrylonitrile. These may be used alone or in combination of two or more. A particularly preferred vinyl monomer is methyl methacrylate. The vinyl monomer is preferably contained in a proportion of 5 to 70% by weight with respect to 30 to 95% by weight of the composite rubber.
[0060]
The composite rubber-based graft copolymer (C) is obtained by adding a composite rubber-based graft copolymer latex obtained by adding the above-mentioned vinyl-based monomer to the above-mentioned composite rubber latex and polymerizing it in one or more stages by radical polymerization technology. It can be separated and recovered by putting it in hot water in which a metal salt such as calcium chloride or magnesium sulfate is dissolved, salting out and solidifying.
[0061]
Such a composite rubber-based graft copolymer (C) is commercially available, for example, as Metabrene S-2001 from Mitsubishi Rayon Co., Ltd.
[0062]
Component (C) is used in an amount of 0.5 to 40 parts by weight, preferably 0.5 to 30 parts by weight, based on 100 parts by weight of component (A). When the amount is less than the above range, the effect of the present invention is not exhibited. When the amount is more than the above range, the rigidity is lowered.
[0063]
As the component (D) phosphate ester compound used in the present invention, the following formula (Formula 11):
[0064]
Embedded image
Figure 0003675493
(Where R1, R2, RThreeAnd RFourEach independently represents a hydrogen atom or an organic group,1= R2= RThree= RFourExcept for = H. X represents a divalent or higher valent organic group, p is 0 or 1, q represents an integer of 1 or more, for example, 30 or less, and r represents an integer of 0 or more. )
The phosphate ester type compound shown by these is mentioned. However, it is not limited to these.
[0065]
In the above formula, examples of the organic group include an alkyl group, a cycloalkyl group, and an aryl group that may or may not be substituted. In addition, when substituted, examples of the substituent include an alkyl group, an alkoxy group, an alkylthio group, a halogen, an aryl group, an aryloxy group, an arylthio group, a halogenated aryl group, and the like. A combined group (for example, an arylalkoxyalkyl group) or a group in which these substituents are combined by an oxygen atom, a sulfur atom, a nitrogen atom, or the like (for example, an arylsulfonylaryl group) may be used as a substituent. Good. The divalent or higher organic group means a divalent or higher valent group formed by removing one or more hydrogen atoms bonded to a carbon atom from the above organic group. Examples include alkylene groups, and preferably (substituted) phenylene groups, polynuclear phenols such as those derived from bisphenols, and the relative positions of the two or more free valences are arbitrary. Particularly preferred are hydroquinone, resorcinol, diphenylolmethane, diphenyloldimethylmethane, dihydroxydiphenyl, p, p'-dihydroxydiphenylsulfone, dihydroxynaphthalene and the like.
[0066]
Examples of specific phosphate ester compounds include trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, tributoxyethyl phosphate, triphenyl phosphate, tricresyl phosphate, cresyl phenyl phosphate, octyl diphenyl phosphate, diisopropyl Phenyl phosphate, tris (chloroethyl) phosphate, tris (dichloropropyl) phosphate, tris (chloropropyl) phosphate, bis (2,3-dibromopropyl) -2,3-dichloropropyl phosphate, tris (2,3-dibromopropyl) Phosphate and bis (chloropropyl) monooctyl phosphate, R1~ RFourPolyphosphates such as bisphenol A bisphosphates, hydroquinone bisphosphates, resorcin bisphosphates, trioxybenzene triphosphates, where is an alkoxy such as methoxy, ethoxy and propoxy, or preferably (substituted) phenoxy such as phenoxy, methyl (substituted) phenoxy Among them, triphenyl phosphate and various polyphosphates are preferable.
[0067]
The component (D) is added in an amount of 1 to 30 parts by weight, preferably 3 to 20 parts by weight, based on 100 parts by weight of the total of the components (A) to (C). When the amount of the component (D) is less than the above range, the effect of the present invention is not sufficiently exhibited, and when it is more than the above range, the heat resistance is impaired.
[0068]
The resin composition of the present invention can further contain an anti-dripping agent. The fluorinated polyolefin that can be used as such an anti-drip agent can be obtained commercially or can be produced by a known method. It can, for example, produce tetrafluoroethylene at a pressure of 100 to 1000 psi and a temperature of 0 to 200 ° C, preferably 20 to 100 ° C in an aqueous medium using a free radical catalyst (eg sodium peroxydisulfate, potassium or ammonium). It is a white solid obtained by polymerization. For details, see Brukerer US Pat. No. 2,393,967. Although not indispensable, it is preferable to use a resin in the state of relatively large particles, for example, particles having an average particle size of 0.3 to 0.7 mm (mainly 0.5 mm). This is better than normal polytetrafluoroethylene powder having a particle size of 0.05 to 0.5 mm. The reason why such a relatively large particle size material is particularly preferred is that it tends to disperse easily in the polymer and bind the polymers together to make a fibrous material. Such a suitable polytetrafluoroethylene is called Type 3 according to ASTM and is actually commercially available as Teflon 6 from E.I. Dupont de Nemours and Company. Alternatively, it can be obtained commercially as Teflon 30J from Mitsui DuPont Fluorochemicals. The fluorinated polyolefin is preferably used in an amount of 0.01 to 2 parts by weight, more preferably 0.05 to 1.0 parts by weight, based on 100 parts by weight of the component (A).
[0069]
In the resin composition of the present invention, in addition to the above-mentioned components, other conventional additives such as pigments, dyes, reinforcements, etc., may be used at the time of resin mixing and molding depending on the purpose, as long as the physical properties are not impaired. Agent (glass fiber, carbon fiber, etc.), filler (carbon black, silica, titanium oxide, etc.), heat-resistant agent, oxidative degradation inhibitor, weathering agent, lubricant, mold release agent, crystal nucleating agent, plasticizer, fluidity improvement An agent, an antistatic agent or the like can be added.
[0070]
There is no restriction | limiting in particular in the method for manufacturing the resin composition of this invention, A normal method can be used satisfactorily. However, the melt mixing method is generally desirable. A small amount of solvent can be used, but is generally not necessary. Examples of the apparatus include an extruder, a Banbury mixer, a roller, a kneader and the like, which are operated batchwise or continuously. The mixing order of the components is not particularly limited.
[0071]
【Example】
The following examples further illustrate the present invention. In the examples, the following components were used.
component (A-1)
RS-PC: copolymerized polycarbonate produced as follows;
Bisphenol A (Nippon GE Plastics Co., Ltd.) 0.22 Kmol, Resorcin 0.22 Kmol and Diphenyl carbonate (Any) 0.44 Kmol are charged into a first tank type agitator (capacity 250 liters), Melted at 140 ° C. While maintaining this temperature, the obtained mixture was fed to the second tank type stirrer (capacity 50 liters) at a rate of 0.16 kilomoles per hour in terms of bisphenol A. The temperature of the 2nd tank type stirrer was hold | maintained at 180 degreeC.
[0072]
As catalysts, tetramethylammonium hydroxide was 0.04 mol / hour and sodium hydroxide was 0.00016 mol / hour (1 × 10 10-6Mol / mol-bisphenol A) was added, the time was adjusted so that the residence time was 30 minutes, and the mixture was stirred.
[0073]
Next, this reaction solution was fed to a third tank type stirrer (capacity 50 liters) at a rate of 0.16 kmol / h in terms of bisphenol A. The temperature of the third tank type agitator was 210 ° C., and the pressure was 200 mmHg. The time was adjusted so that the residence time was 30 minutes, and the mixture was stirred while extracting and removing phenol.
[0074]
Next, this reaction solution was fed to a fourth tank type stirrer (capacity 50 liters) at a rate of 0.16 kmol / h in terms of bisphenol A. The temperature of the 4th tank type stirrer was 240 degreeC, and the pressure was 15 mmHg. The time was adjusted so that the residence time was 30 minutes, and the mixture was stirred while extracting and removing phenol. The intrinsic viscosity [η] of the reaction product obtained after the reaction became steady was 0.15 dl / g.
[0075]
Next, the reaction product was pressurized with a gear pump and sent to a centrifugal thin film evaporator at a rate of 0.16 km / hr in terms of bisphenol A to proceed the reaction. The temperature and pressure of the thin film evaporator were controlled at 270 ° C. and 2 mmHg, respectively. The reaction product was placed in a biaxial horizontal stirring polymerization tank (L / D = 3, stirring blade rotating diameter 220 mm, internal volume 80 liters) controlled at 290 ° C. and 0.2 mmHg with a gear pump from the bottom of the evaporator. Conversion was performed at a rate of 0.16 kilomoles per hour (about 40 kg / hour), and polymerization was carried out with a residence time of 30 minutes. The intrinsic viscosity [η] of the product at this time was 0.49 dl / g. The product was a copolymerized polycarbonate having the following formulas (Chemical Formula 12) and (Chemical Formula 13) in a molar ratio of 50:50. Hereinafter, this is abbreviated as RS-PC.
[0076]
Embedded image
Figure 0003675493
[0077]
Embedded image
Figure 0003675493
PC (1): Polycarbonate of bisphenol A (trademark; Lexan, manufactured by GE Plastics Co., Ltd.), intrinsic viscosity of 0.56 dl / g measured at 25 ° C. in methylene chloride
PC (2): Polycarbonate of bisphenol A (trademark; Lexan, manufactured by GE Plastics Co., Ltd.), intrinsic viscosity of 0.50 dl / g measured in methylene chloride at 25 ° C
PC (3): Polycarbonate of bisphenol A (trademark; Lexan, manufactured by GE Plastics Co., Ltd.), intrinsic viscosity measured at 25 ° C. in methylene chloride 0.44 dl / g
component (A-2)
SAN resin: Trademark SR 30B (manufactured by Ubesaikon Co., Ltd.)
Ingredient (B)
ABS resin: Trademark UX 050 (manufactured by Ubesaikon Co., Ltd.)
Ingredient (C)
METABLEN S-2001: Trademark, methyl methacrylate-butyl acrylate-dimethylsiloxane copolymer, manufactured by Mitsubishi Rayon Co., Ltd.
Ingredient (D)
CR733S: Trademark, phenyl resorcinol polyphosphate, manufactured by Daihachi Chemical Co., Ltd.
Optional ingredients
Teflon 30J: Trademark, polytetrafluoroethylene, manufactured by Mitsui DuPont Fluorochemicals
Example 1 and Comparative Examples 1 to 4
Each component was mixed in the ratio (weight ratio) shown in Table 1 and extruded with a twin-screw extruder (30 mm) set at 240 ° C. and 150 rpm to prepare pellets. The pellets were then injection molded at a set temperature of 250 ° C and a mold temperature of 60 ° C. The obtained molded product was measured for Izod impact strength and melt index (MI) to evaluate flame retardancy. The results are shown in Table 1.
[0078]
In addition, the evaluation test of the resin composition was performed as follows.
(1) Izod impact strength (Kg-cm / cm)
Measured according to ASTM D 256 with a thickness of 1/8 inch and notched.
(2) Melt index (MI)
According to ASTM D 1238, measurement was performed at a temperature of 260 ° C. and a load of 5 kg.
(3) Flame resistance test
UL94 / V0, VI, VII test
Five test bars were tested at a thickness of 1/16 inch according to the test method shown in Bulletin 94 “Burn Test for Material Classification” (hereinafter referred to as UL-94) of Underwriters Laboratories, Inc. According to this test method, the material under test was rated to one of UL-94 V-0, V-I and V-II based on the results of five samples. The criteria for each V grade for UL-94 is roughly as follows.
V-0: The average flame holding time after removing the ignition flame is 5 seconds or less, and all the samples do not drop the fine flame that ignites the absorbent cotton.
V-I: The average flame holding time after removing the ignition flame is 25 seconds or less, and all the samples do not drop the fine flame that ignites the absorbent cotton.
V-II: The average flame holding time after removing the ignition flame is 25 seconds or less, and these samples drop the particulate flame that ignites absorbent cotton.
[0079]
In addition, UL-94 stipulates that if all test bars do not pass a specific V grade, they should not be classified into that grade. If this condition is not met, the five test bars are given the grade of the one with the worst performance. For example, if one test bar is classified as V-II, the grade for all five test bars is V-II.
UL94 / 5V (5VB) test (5 inch flam test)
Using method A (bar test), place the test piece 5 times on the burner, (1) burning time and glowing time, (2) burning distance of the test piece, (3) presence or absence of dripping material (drip), ( 4) Deformation and physical strength were observed. Note that the thickness of the test piece was 2.5 mm. Criteria for passing 5VB: The burning time and / or glowing after 5 test flames are applied to any test piece does not exceed 60 seconds. And none of the test pieces are dripping.
[0080]
[Table 1]
Figure 0003675493
[0081]
【The invention's effect】
According to the present invention, it is possible to provide a polycarbonate-based resin composition that is remarkably excellent in flame retardancy even when molded thinly. In particular, the resin composition of the present invention has a high dripping suppression effect. Therefore, the resin composition of the present invention is very useful industrially.

Claims (5)

(A)(A-1) 次式(化1):
Figure 0003675493
および次式(化2):
Figure 0003675493
(上記式中、R4 およびR5 はそれぞれ独立して、ハロゲン原子または一価の炭化水素基であり、Bは−(R1 −)C(−R2 )− [ここで、R1 およびR2 はそれぞれ独立して水素原子または1価の炭化水素基である]、−C(=R3 )− [ここでR3 は2価の炭化水素基である]、−O−、−S−、−SO−または−SO2 −であり、R6 は炭素数1〜10の炭化水素基もしくはそのハロゲン化物またはハロゲン原子であり、p、qおよびnはそれぞれ独立して0〜4の整数である)
で示される構造単位を有し、かつ前記(化2)の構造単位の量は(化1)および(化2)の構造単位の合計量の2〜90モル%を占めるところの共重合ポリカーボネートまたはこれとポリカーボネート系樹脂1〜100 重量部、ならびに
(A-2) (a) 芳香族ビニル単量体成分および(b) シアン化ビニル単量体成分を、共重合体の構成成分として含む共重合体99〜0重量部を含み、かつ、(A)100重量部に対して、
(B)(a) 芳香族ビニル単量体成分、(b) シアン化ビニル単量体成分および(c) ゴム質重合体を、共重合体の構成成分として含む共重合体0.5 〜40重量部ならびに
(C)ポリオルガノシロキサンおよびポリアルキル(メタ)アクリレートを含む複合ゴムにビニル系単量体がグラフトしてなる複合ゴム系グラフト共重合体0.5 〜40重量部を含み、さらに(A)〜(C)の合計100重量部に対して、
(D)リン酸エステル系化合物1〜30重量部を含む難燃性樹脂組成物。
(A) (A-1) The following formula (Formula 1):
Figure 0003675493
And the following formula (Formula 2):
Figure 0003675493
(In the above formula, R 4 and R 5 are each independently a halogen atom or a monovalent hydrocarbon group, and B is — (R 1 —) C (—R 2 ) — [where R 1 and R 2 is each independently a hydrogen atom or a monovalent hydrocarbon group], —C (═R 3 ) — [wherein R 3 is a divalent hydrocarbon group], —O—, —S —, —SO— or —SO 2 —, R 6 is a hydrocarbon group having 1 to 10 carbon atoms, a halide thereof, or a halogen atom; p, q and n are each independently an integer of 0 to 4; Is)
And the amount of the structural unit of (Chemical Formula 2) occupies 2 to 90 mol% of the total amount of the structural units of (Chemical Formula 1) and (Chemical Formula 2) or 1 to 100 parts by weight of this and polycarbonate resin, and
(A-2) containing 99 to 0 parts by weight of a copolymer containing (a) an aromatic vinyl monomer component and (b) a vinyl cyanide monomer component as a constituent of the copolymer, and ( A) For 100 parts by weight,
(B) (a) aromatic vinyl monomer component, (b) vinyl cyanide monomer component, and (c) a copolymer containing 0.5 to 40 parts by weight of a rubbery polymer as a constituent of the copolymer And (C) 0.5 to 40 parts by weight of a composite rubber graft copolymer obtained by grafting a vinyl monomer to a composite rubber containing polyorganosiloxane and polyalkyl (meth) acrylate, and (A) to (A C) for a total of 100 parts by weight,
(D) A flame retardant resin composition containing 1 to 30 parts by weight of a phosphoric ester compound.
成分(A)の(A-1) において、式(化1)および(化2)中のBが−(R1 −)C(−R2 )− (R1 およびR2 は上記と同義である)で示される請求項1記載の樹脂組成物。In the component (A) (A-1), B in the formulas (Chemical Formula 1) and (Chemical Formula 2) is — (R 1 —) C (—R 2 ) — (R 1 and R 2 are as defined above). The resin composition according to claim 1, which is represented by: 成分(A)において、(A-1) 10〜99重量部に対して(A-2) が90〜1重量部配合される請求項1または2記載の樹脂組成物。  3. The resin composition according to claim 1, wherein in component (A), 90 to 1 part by weight of (A-2) is blended with 10 to 99 parts by weight of (A-1). 成分(B)において、(b−1)がABS樹脂、AES樹脂、ACS樹脂およびAAS樹脂から選択され、かつ(b−2)がSAN樹脂である請求項1〜3のいずれか1項記載の樹脂組成物。  The component (B), wherein (b-1) is selected from ABS resin, AES resin, ACS resin and AAS resin, and (b-2) is a SAN resin. Resin composition. 成分(D)リン酸エステル系化合物が、次式(化3):
Figure 0003675493
(ここで、R1 、R2 、R3 およびR4 は、それぞれ独立して、水素原子または有機基を表すが、R1 =R2 =R3 =R4 =Hの場合を除く。Xは2価以上の有機基を表し、pは0または1であり、qは1以上の整数、rは0以上の整数を表す。)
で示される化合物である請求項1〜4のいずれか1項記載の樹脂組成物。
The component (D) phosphate ester compound has the following formula (Formula 3):
Figure 0003675493
(Wherein R 1 , R 2 , R 3 and R 4 each independently represents a hydrogen atom or an organic group, except for R 1 = R 2 = R 3 = R 4 = H. X Represents an organic group having 2 or more valences, p is 0 or 1, q represents an integer of 1 or more, and r represents an integer of 0 or more.)
The resin composition according to claim 1, which is a compound represented by the formula:
JP35353293A 1993-12-28 1993-12-28 Flame retardant resin composition Expired - Lifetime JP3675493B2 (en)